Jiangxi Engineering Laboratory of Waterborne Coating, Department of Coatings and Polymeric Materials, School of Chemistry and Chemical Engineering, Jiangxi Science and Technology Normal University, Nanchang 330013, P. R. China. E-mail: jiangzhong@jxstnu.com.cn; liangshen@jxstnu.com.cn; hehf0427@jxstnu.com.cn
First published on 13th November 2020
In this paper, large-scale, self-standing polypyrrole/graphene oxide (PPy/GO) nanocomposite films were prepared by an environmentally friendly and easy-to-operate confined polymerization method, and were also assembled as electrode materials for symmetric all-solid-state supercapacitors. In this paper, large-scale, self-standing polypyrrole/graphene oxide (PPy/GO) nanocomposite films were prepared by an environmentally friendly and easy-to-operate confined polymerization method, and were also assembled as electrode materials for symmetric all-solid-state supercapacitors. The morphology, chemical structure and electrochemical property were characterized by field emission scanning electron microscope (FESEM), Fourier transform infrared spectroscopy (FTIR), cyclic voltammetry (CV), galvanostatic charge–discharge (GCD), and electrochemical impedance spectroscopy (EIS), respectively. The lamellar structure of GO and both strong interaction with ice and pyrrole could promote polymerization of pyrrole and improve the compactness of the film. With the aid of GO, the conjugation length of PPy increased, the resistance of the material decreased, and the electrochemical energy storage of the composite film was significantly enhanced. In the case of 2.5 wt% GO, the prepared PPy/GO nanocomposite supercapacitor exhibited a high area specific capacitance of 97.3 mF cm−2 at 1 mA cm−2. Furthermore, the PPy/GO film supercapacitor also showed excellent cycling stability and good flexibility.
Graphene with its excellent electrical conductivity, high specific area and superior mechanical properties, has drawn intense attention in enhancing the electrochemical performance of PPy.22 Biswas and Drzal constructed a multilayer nanostructured supercapacitor with high specific capacitance through π–π interaction between PPy nanowires and graphene nanosheets.23 Though, graphene is difficult to disperse evenly in aqueous solution owing to its hydrophobic and easy agglomeration. Shu et al. reported a so-called “Tandem” strategy to fabricate flexible graphene/PPy nanofiber film using surfactant to exfoliate expanded graphite and as a template for the growth of PPy nanofiber.24 In addition, chemical modification of graphene is a common method to improve its dispersion, such as graphene oxide (GO). Konwer et al. prepared the PPy/GO electrode materials by in situ polymerization, which exhibited a improved electrical conductivity.25 Lv et al. developed a one-step electrosynthesis of PPy/GO composites using GO as the anionic dopant.26 Moreover, many efforts have been explored to fabricate film electrode materials for flexible devices, such as soft template assistance,27 vacuum filtration,8,24 electrochemical polymerization,28,29 and interfacial polymerization.30 However, these methods are usually cumbersome, costly, or unfriendly. Therefore, the large-scale preparation of highly efficient and controllable, low-cost, and environmentally friendly PPy/GO films electrode materials remains a challenge.
Herein, an environmentally friendly and easy-to-operate confined polymerization inside the ice method was exploited to successfully synthesize PPy/GO films with a diameter of 8 cm. The interaction between pyrrole monomer/GO and solid ice/alcohol surface formed at low temperature, resulting in two-dimensional polymerization. The prepared composites films were then assembled to solid supercapacitors. The cyclic voltammetry, galvanostatic charge/discharge, and electrochemical impedance spectroscopy measurements were employed to characterize their energy storage behaviors. The results showed that the electrodes of self-standing PPy/GO films prepared by this novel method exhibited excellent electrochemical performance, which provided a good feasible strategy for all-solid-state supercapacitors.
![]() | (1) |
![]() | (2) |
![]() | (3) |
![]() | ||
Fig. 2 Schematic illustration of self-standing PPy/GO film: (i) smooth ice, (ii) pyrrole/GO layer, (iii) PPy/GO layer. |
Fig. 3 shows the FTIR spectra of the PPy and PPy/GO-1.0, PPy/GO-1.5, PPy/GO-2.0, PPy/GO-2.5 samples. The characteristic peaks located at 1466 and 1544 cm−1 were assigned to the symmetric and asymmetric ring-stretching modes of pyrrole, respectively.34 The C–H in-plane bending and out-of-plane bending were observed at 1182 and 912 cm−1.16 The peaks at 1300 and 1386 cm−1 were due to the C–C and C–N stretching vibrations, respectively.35 Obviously, with the addition of GO, the C–N stretching vibrations peak was downshifted to 1377 cm−1 probably because of the π–π interactions and hydrogen bonding between the GO layers and aromatic PPy rings.36,37 Additionally, the ratio between the peak area of the symmetric ring stretching mode and asymmetric ring stretching mode (I1466/I1544) could be used to calculate the conjugation length.35,38 The ratio was increasing from 0.583 to 0.681, 0.719, 0.815, 0.969 for PPy, PPy/GO-1.0, PPy/GO-1.5, PPy/GO-2.0, PPy/GO-2.5, respectively, which suggested that the conjugation length increased with further addition of GO. The reason might be that the strong interfacial interaction between PPy and GO induced more electrons delocalized either in the pyrrole units or the benzene ring units of GO.35,39
Fig. 4 shows the SEM images of PPy and PPy/GO films. From Fig. 4a, the neat PPy film displayed a smooth morphology, but there were some holes in it, probably due to the penetration of pyrrole monomers in the pores of ice. With the addition of GO, the film became denser, and a few particles appeared on the surface (Fig. 4b). If the content of GO increased, the lamellar structure of GO could be observed (Fig. 4c). Meanwhile, at the higher content, the individual GO sheets attached to PPy could be obviously found (Fig. 4d and e). These results suggested that GO played an important role in the morphology of the films. On the one hand, the nanosheet structure of GO and its strong interaction with pyrrole led to more pyrrole on the surface, thus promoting polymerization.40 On the other hand, the lamellar characteristics of GO and its strong hydrogen bond with the ice layer could effectively prevent pyrrole molecules from infiltrating ice layer. The measurement of water contact angles was performed to investigate the roughness of material surface, as shown in Fig. 4f and insets of Fig. 4a–e. The water contact angle of the composite film increased gradually with the increase of GO content, indicating the increase in the surface roughness of the film. As mentioned above, more PPy particles formed on the surface, thus the surface roughness increased.
Fig. 5 exhibits the CV curves of FSCs devices at different scan rates. The CV curve is closer to the rectangle and more symmetrical, indicating better capacitance performance of the material.41 In Fig. 5a–e, the quasi-rectangular shape appeared in all as-prepared supercapacitor at low scan rates, which confirmed that the PPy and PPy/GO nanocomposite self-supporting films displayed good ionic and electronic transport. At the same time, as the scan rate increased, the highly distorted leaf-shaped CV curves were observed, indicating deviation from the ideal capacitance response, which was consistent with the characteristics of conductive polymer-based supercapacitors.3 With the increase of GO content, the area of CV curves of PPy/GO supercapacitors increased in comparation with the PPy supercapacitor, suggesting the enhancement in capacitance.
![]() | ||
Fig. 5 The CV behaviors of solid-state supercapacitors (a) FSC-1, (b) FSC-2, (c) FSC-3, (d) FSC-4, (e) FSC-5 at different scan rates. (g) Nyquist plots of the FSCs devices. |
The EIS method is a powerful method to understand the whole electrochemical environment for a meaningful analysis.42 As shown in Fig. 5g, the Nyquist plots of FSCs consisted of a semicircle in the high frequency region and a straight line in the low frequency region. The former semicircle diameter represented the interfacial charge transfer resistance, while the slope of the latter straight line indicated the capacitive property.43,44 The semicircle diameter of FSC-4 was smallest in the high frequency region, indicating the easier electron transfer in the PPy/GO-2.5 film. The inset of Fig. 5g shows the equivalent electrical circuit, where Re is equivalent series resistance (ESR), Rct is the charge transfer resistance, Zw is the Warburg element, Cdl and Cps are the constant phase element (the double layer capacitance and pseudocapacitance), respectively. The PPy showed a comparatively high ESR of 22.4 Ω, whereas the PPy/GO-1.0, PPy/GO-1.0-1.5, PPy/GO-2.0, and PPy/GO-2.5 nanocomposites film exhibited the ESR of 15.23 Ω, 11.11 Ω, 8.84 Ω, and 4.12 Ω. The low ESR of PPy/GO suggested an enhancement of electrical conductivity on the incorporation of GO, which might be attributed to the following reasons. On the one hand, perhaps GO could be partial reduction during in situ polymerization to improve conductivity.45 On the other hand, the conjugation length of PPy could be increasing under the influence of GO, resulting in conducting particle delocalization more easily.35 The improved electrical conductivity facilitated rapid charge transport at the interface, leading to better energy storage behaviors.8,44 Moreover, the straight line in the frequency region was closer to Y axis for PPy/GO supercapacitors, signifying ideal supercapacitor performance due to the synergistic effect of PPy/GO, which was consistent with the results of CV curves.
For quantitative evaluation of charge storage capacity, we investigated the GCD performance of FSCs supercapacitors at different current densities, as shown in Fig. 6. The GCD curves of FSCs supercapacitor were almost symmetrical, indicating their good capacitance behaviors. Meanwhile, as the current density increased, the capacitance of all FSCs samples decreased, which was also in agreement with results of CV measurements. It was worth noting that the IR drop of FSC-5 was minimal, confirming its low internal resistance and less energy loss during charge/discharge process.33 Fig. 6f shows the calculated areal specific capacitances of FSCs at different current densities according to the GCD profile. A highest area specific capacitance of 97.3 mF cm−2 was obtained at 1 mA cm−2 for FSC-5 supercapacitor. The other samples introduced with GO, FSC-2 (34.6 mF cm−2), FSC-3 (46.1 mF cm−2) FSC-4 (68.9 mF cm−2) also exhibited higher area specific capacitance than FSC-1 (13.89 mF cm−2). The Ragone plots are shown in Fig. 7. The calculated energy densities according to eqn (2) were 1.8, 4.1, 6.4, 9.6 and 13.56 μW h cm−2 at a power density of 0.5 mW cm−2 for FSC-1, FSC-2, FSC-3, FSC-4, and FSC-5, respectively. The higher content of GO, the better energy storage performance. The GO nanosheets with high surface area not only improved the film forming performance, but also effectively enhanced the conjugation length of PPy, resulting in decrease of resistance of electrode material and increase of charge transport capacity.8,43,46,47
![]() | ||
Fig. 6 GCD profiles of (a) FSC-1, (b) FSC-2, (c) FSC-3, (d) FSC-4, and (e) FSC-5 at different current densities. (f) The plots of areal specific capacitance for FSCs. |
The cycle life was also an important indicator for evaluating supercapacitor performance. Fig. 8a illustrates the cycle life of the FSC-1 and FSC-5 supercapacitors at a current density of 1 mA cm−2. It could be observed that the capacitance of FSC-1 decreased rapidly, while the FSC-5 remained a stable capacitance after 1000 charge/discharge cycles. The areal specific capacitance of FSC-5 dropped only 6%, whereas the FSC-1 lost 55% of capacitance. The volumetric swelling and contraction of the PPy chain during the doping/dedoping (charge/discharge) process significantly influenced the charge distribution and conformation of π conjugated polymer chains, leading to a decline in charge storage capacity. For PPy/GO film, the good electrochemical stability and mechanical strength of GO as the “skeleton” in the composite film could reduce the volume change of PPy chains, thus delaying the degradation of PPy chain and the attenuation of the capacitance.7,23 It was well known that ideal supercapacitors should be adapt to any operating conditions. Therefore, it was of great significance to investigate the electrochemical properties of supercapacitors under bending conditions. Fig. 8b shows the GCD diagrams of the FSC-5 capacitor at different bending angles. The GCD curves with little variation at different bending angles indicated that the prepared FSC-5 possessed the characteristics of flexibility and portability.
![]() | ||
Fig. 8 (a) Cycling behaviors of FSC-1 and FSC-5 symmetric supercapacitor. (b) GCD curves of FSC-5 with different bending angles at a current density of 1 mA cm−2. |
Footnote |
† Jia Wen and Yang Ding contributed equally to this work. |
This journal is © The Royal Society of Chemistry 2020 |