Hanan H. Ibrahim,
Adel A. Mohamed and
Ismail A. M. Ibrahim*
Department of Chemistry, Faculty of Science, Helwan University, 11795 Cairo, Egypt. E-mail: ismail.ibrahim@science.helwan.edu.eg
First published on 26th November 2020
The characteristic properties of TiO2 (anatase) make doping necessary to enhance its photocatalytic activity. Herein, a density functional theory (DFT) study using the Heyd–Scuseria–Ernzerhof (HSE) hybrid functional was performed to precisely investigate the effect of mono- and co-doping (Ni, Se and B) on the structural, electronic and optical properties of anatase TiO2. Notably, the origin of the enhanced photocatalytic activity of the modified systems was determined. The response to visible light was enhanced for all the mono- and co-doped materials except for Bint, and the highest absorption coefficient was observed for Se4+ mono-doping and Se/Bint+sub and Ni/Bsub co-doping. The decrease in bandgap is associated with a red shift in the absorption edges with the smallest bandgap calculated for Ni/Bsub (2.49 eV). Additionally, the Ni, Se4+ and Se2− mono-doped systems and Ni/Se4+ co-doped systems are proposed as promising photocatalysts for water splitting applications and further experimental validation. Moreover, the Ni/Bint+sub and Se/Bint+sub co-doped materials can also be valuable photocatalysts for other energy applications due to their enhanced visible light activity and the prolonged lifetime of their produced charge carriers.
Nickel doping was largely exhibited since the ionic radius of Ni2+ ions is slightly higher than that of Ti4+ ions.9 Several experimental methods have been employed for the synthesis of Ni-doped TiO2 such as the electrospinning technique,12 co-precipitation method,13 hydrothermal method,14 and sol–gel method.15 The visible light response and enhanced photocatalytic performance of Ni-doped anatase have been extensively reported.14,16 Based on diffuse reflectance spectroscopy (DRS) analysis, bandgap narrowing increases as a function of the dopant concentration.14,16 Quantum mechanical methods based on density functional theory were used to explain the optical response and changes in the electronic properties of TiO2 upon Ni doping.17 On the other hand, several reports on selenium doping were recently published, suggesting that it exhibits several oxidation states, including Se4+, Se0 and Se2−.18 Although, cationic Se4+ and Se0 have been significantly assigned experimentally, Se2− was only clarified theoretically in the previous work by Harb.10 Xie et al. attributed the narrowed gap (2.19 eV) and the suppressed electron/hole recombination rate upon Se4+ doping to the energy states appearing in the gap region upon the incorporation of Se.11 A DFT-based study with HSE level showed the effect of Se doping at different valence states with different concentrations on water splitting.10 The results showed that substitutional cationic and anionic Se can induce the best band positions for the water splitting reaction. Nonetheless, substitutional Se2− within the same crystal provides localized gap states capable of limiting the hole mobility and enlarging the recombination rate.10
For boron-doped TiO2, it was found that B doping has photochemical19,20 and electrochemical applications,21 such as degradation of atrazine as an organic pollutant on light absorption and high performance anode for sodium ion batteries. Based on previous experimental and theoretical studies, B can occupy different sites in the crystal lattice of anatase TiO2, either interstitial or substitutional sites, and at high concentration it can occupy both sites.20 For interstitial B, no visible light activity was observed; however, a response to visible light was detected for substitutional B due to the electronic transitions from the deep states.22,23 At high concentration, both interstitial and substitutional B were found to be stable in bulk anatase or co-doped with other elements.20,23 B was co-doped with Ni by Masae et al., who claimed the improvement of photocatalytic activity upon co-doping, but the origin of this enhancement was not clear.24
To the best of our knowledge, neither Ni/Se co-doping nor Se/B co-doping has been addressed experimentally and theoretically to date. Therefore, this study proposes new co-doped TiO2 photocatalysts for further experimental validation. In the current work, we attempted to study the effect of mono-doping and co-doping with different metals and non-metals at the HSE hybrid functional level on the photocatalytic activity of anatase TiO2. In our calculations, the structural, electronic, and optical properties were addressed and compared to the available experimental data. In addition, a systematic description of the induced levels on defect formation and the interaction between these states on co-doping were exhibited. Besides, the formation energy was also calculated, revealing the stability upon the introduction of the dopant to the anatase lattice. We found that most dopants reduced the bandgap, with a significant improvement for co-doped materials. The visible light response and the value of the absorption edge were determined from UV-Vis absorption spectra calculated at the HSE hybrid functional level together with the frequency-dependent dielectric function. The photocatalytic reaction of TiO2-based materials was investigated by determining the band edge position of modified materials with respect to the normal hydrogen electrode (NHE) potential for water splitting.
System | Lattice parameter | Cell volume (Å3) | ΔV (Å3) | |
---|---|---|---|---|
a (Å) | c (Å) | |||
Pure TiO2 | 3.835 (3.784) | 9.624 (9.502) | 1273.91 | — |
Ni–TiO2 | 3.838 (3.789) | 9.631 (9.715) | 1276.78 | 2.78 |
Se4+–TiO2 | 3.839 (3.760) | 9.633 (9.490) | 1277.62 | 3.71 |
Se2−–TiO2 | 3.851 | 9.665 | 1290.13 | 16.22 |
Bsub–TiO2 | 3.842 | 9.642 | 1280.83 | 6.92 |
Bint–TiO2 | 3.846 | 9.652 | 1285.14 | 11.23 |
Bint+sub–TiO2 | 3.851 | 9.664 | 1289.90 | 15.99 |
Ni/B–TiO2 | 3.840 | 9.637 | 1278.91 | 5.00 |
Ni/Bint+sub–TiO2 | 3.851 | 9.665 | 1290.33 | 16.42 |
Se4+/B–TiO2 | 3.849 | 9.659 | 1287.71 | 13.80 |
Se4+/Bint+sub–TiO2 | 3.864 | 9.699 | 1303.85 | 29.94 |
Ni/Se4+–TiO2 | 3.838 | 9.631 | 1276.69 | 2.78 |
Ni/Se2−–TiO2 | 3.851 | 9.663 | 1289.55 | 15.64 |
Fig. 1 Optimized geometries of (a) Ni-doped, (b) Se4+-doped, (c) Se2−-doped, (d) Bsub-doped, (e) Bint-doped, and (f) Bint+sub-doped anatase TiO2 determined using the HSE hybrid functional level. |
In the case of the mono-doped materials, the replacement of Ti4+ by Ni2+ leads to the formation of oxygen vacancy to preserve the charge neutrality, showing a stoichiometry of NixTi1−xO2−δ where (x = 0.028 and δ = 0.028), and the relaxed geometry is shown in Fig. 1a. The calculated Ni–O bond length is 2.06 Å, which is slightly longer than the reference Ti–O bond due to the ionic radii differences. The calculated PDOS of the Ni mono-doped anatase (Fig. 2b) shows hybridization between the Ni 3d and O 2p states, which confirms the existence of an Ni–O–Ti bond. The incorporation of Ni into the anatase TiO2 lattice preserves the diamagnetism of the system with a singlet spin state and a magnetic moment of 0 μB.39 Moreover, it can be observed that the Ni states are completely overlapped with the VBM, with some states located at 2.53 eV from the CBM. Therefore, the main bandgap is reduced to 2.89 eV with an energy gap of 2.53 eV, which is consistent with the previous results by Blanco-Vega et al.15 for Ni doped at small concentrations. Thus, based on the bandgap reduction, enhanced photoactivity towards visible light can be observed upon Ni mono-doping.
For Se-modified anatase, substitutional Se is doped at two different sites with two different stoichiometries.18 In one structure, Se4+ is substituted at the Ti4+ site with the formula of SexTi1−xO2, whereas Se2− at the oxygen site leads normally to TiO2−δSeδ. For the configuration with cationic Se, the obtained Se–O bond has a length of 2.00 Å, whereas the Ti–Se bond formed upon anionic Se doping of 2.30 Å is much longer. For both cases, a closed-shell singlet spin state was observed, corresponding to the diamagnetic properties of the formed structures. The DOS and PDOS for the cationic Se depicted in Fig. 2c shows a slight increase (0.03 eV) in the main bandgap value on the formation of the Se4+ defect; however, the energy gap originating from the incorporation of Se states in the bandgap region is about 2.18 eV. The energy gap calculated for Se4+ mono-doping is consistent with the previously observed value.11,40 The slight increase in the calculated main band gap was reported using the standard HSE06 functional.10 The calculated main bandgap value for two Se4+ doped anatase within the standard HSE06 functional was about 3.4 eV, whereas the calculated bandgap value of pure anatase was 3.3 eV.10 However, as shown in Table 2, Se4+ doping decreases the band gap of TiO2 experimentally.18 This can be attributed to the anatase to rutile phase transition on Se doping, where the anatase percentage was 50% at the calcination temperature of 650 °C.18 The deep states formed in the bandgap region is mainly due to the Se 4s states with a small contribution from the Se 4p states to the valence band (VB).41 However, the Se 4p contribution to the conduction band (CB) is noticeable. Furthermore, the Se 4s states are hybridized with the O 2p states, which gives an indication of the strength of the formed Se–O bond. The doped Se impacts the diamagnetic properties of the modified TiO2, which is associated with the closed shell singlet state, resulting in a 0 μB net magnetic moment. On the other hand, the anionic Se2−-modified anatase structure formed through oxygen substitution reveals different DOS and PDOS from the cationic doped material (Fig. 2d). The main bandgap is reduced to 3.18 eV, while the energy gap is narrowed to 1.88 eV by the Se2− impurity states in the forbidden region.10 The gap states are mainly due to the Se 4p states, which are separated by 2.34 and 1.88 eV from the CBM.41 Some of these states are overlapped with the VBM, while the other states are hybridized with the O 2p states. For both Se mono-doped cases, the electron transition is allowed from the induced bandgap states to the CB. Consequently, the photocatalytic activity of these materials under visible light is enhanced. Nevertheless, the charge separation efficiency may be affected by these deep states, and consequently the photocatalytic activity. Accordingly, it is worthwhile to co-dope these materials with another elements capable of improving the charge separation efficiency.
System | Bandgap (eV) | Exp. bandgap | Energy gap (eV) | Formation energy (Ef) | |
---|---|---|---|---|---|
Ti-rich | O-rich | ||||
Pure TiO2 | 3.26 | 3.20 | 3.26 | — | — |
Ni–TiO2 | 2.89 | 2.72 | 2.53 | 4.579 | 0.118 |
Se4+–TiO2 | 3.29 | 3.05 | 2.18 | 7.911 | −1.011 |
Se2−–TiO2 | 3.18 | 1.88 | 1.155 | 5.616 | |
Bsub–TiO2 | 3.21 | 1.04 | 3.873 | 8.334 | |
Bint–TiO2 | 3.52 | 0.23 | 0.635 | 0.635 | |
Bint+sub–TiO2 | 3.40 | 0.23 | −3.568 | 7.276 | |
Ni/Bsub–TiO2 | 2.49 | 1.10 | 5.921 | 5.291 | |
Ni/Bint+sub–TiO2 | 2.78 | 0.31 | 5.331 | 5.330 | |
Se4+/Bsub–TiO2 | 2.98 | 1.23 | 10.088 | 5.627 | |
Se4+/Bint+sub–TiO2 | 3.31 | 0.26 | 8.512 | 4.050 | |
Ni/Se4+–TiO2 | 2.87 | 2.50 | 11.680 | −1.703 | |
Ni/Se2−–TiO2 | 3.11 | 1.55 | 3.893 | 3.893 |
The B-doped TiO2 was simulated by replacing B2− at the O2− site with the formula of TiO2−δBδ, and inserting B into the anatase lattice, leading to TiO2Bδ. The mixed interstitial-substitutional B system was also modeled through substitution of O2− by B from the anatase supercell with the incorporation of an additional B into the crystal system as TiO2−δB2δ. In the anatase lattice, Bsub is bound to three neighboring Ti ions with three bonds, i.e. two short (2.12 Å) and one long (2.39 Å) bonds (Fig. 1d).22 Boron added to the lattice has an odd number of valence electrons, indicating the paramagnetic properties of the neutral defect. In our study, we considered the doublet spin state, and thus the third electron is shared with a single Ti rather than bonding, explaining the longer bond length. The electrons occupy the hybrid B 2p–Ti 3d states localized deep in the bandgap region at about 1.34 and 1.04 eV for the spin up states and 1.22 eV for the spin down state below the conduction band minimum (CBM). The electronic transitions from these states can occur on visible light absorption; however, these deep states can suppress the carrier separation. Moreover, the main bandgap is slightly red shifted from the anatase bandgap, in agreement with the previous experimental observations.38,42 For interstitial B (Bint), it was reported that Bint may be tricoordinate [BO3] or tetracoordinate [BO4].22 However, the electronic characteristics of interstitial boron were rather independent of the site where the boron atom is incorporated.22 Therefore, we only considered a [BO3] structure in our work, as shown in Fig. 1e. The interstitial B atom is bonded to the three vicinal oxygen ions, where two bonds are similar (1.4 Å) and the third is shorter (1.376 Å). In this case, the boron exhibits a trigonal planer coordination.26 According to the PDOS, as shown in Fig. 2f, it is observed that no states due to boron contribution are formed in the bandgap, while the B 2p states are located below the valence band.22 The states incorporated and overlapped with the CBM are mainly due to the Ti3+ ions, which can trap the photo-generated carriers and enlarge the lifetime of these carries.43 This result indicates that the B electrons are partially delocalized and consequently donated to the lattice forming B3+.22 Despite the Ti3+ states, the main bandgap is blue shifted upon the introduction of interstitial boron, and no visible light response is detected for that system.23,44 The blue-shifted bandgap is attributed to the existence of BOx, which has a high bandgap compared to pure anatase.22,45 The situation for Bint+sub is different since the concentration of B in the lattice is increased by the introduction of two B atoms, i.e. one at an interstitial position and the other at the substitutional position, replacing an oxygen ion from the lattice, as shown in Fig. 1f. With this coupling, the bond lengths change from the mono-doped case. The three bonds surrounding the interstitial B are equal (1.379 Å), whereas the bonds around the substitutional B are still two short and one long bond (2.07 and 2.12 Å), respectively. The PDOS of Bint+sub (Fig. 2g) shows that the gap states move high in the bandgap towards the CB. Moreover, two of the shallow levels seen in Bint almost disappear in Bint+sub by the interaction between Bint and Bsub with overlap between their states. However, one shallow state due to Ti3+ is still observed below the CB, which may be associated with enhanced electron trapping. The main bandgap is slightly red shifted from Bint, but still higher than the anatase bandgap.
On co-doping, the Ni/Bsub, Ni/Bint+sub, Se4+/Bsub, Se4+/Bint+sub, Ni/Se2−, and Ni/Se4+ co-doped systems are associated with NixTi1−xO2−2δBδ, NixTi1−xO2−2δB2δ, SexTi1−xO2−δBδ, SexTi1−xO2−δB2δ, NixTi1−xO2−2δSeδ, and NixSexTi1−2xO2−δ, respectively. For all the co-doped materials, x = 0.028 and δ = 0.028 if they exist. For the co-doping models, different configurations were considered by distributing the dopants (adjacent and separated) in the supercell. It was found that the formation of adjacent dopants is more energetically favorable with respect to other configurations.46 Therefore, the lowest energy structures were selected to examine their electronic and optical properties and their catalytic activity (see ESI† for fractional coordinates). Ni/Bsub co-doping exhibits different ionic features from the mono-doped materials. The PDOS for Ni/Bsub shows an interaction between the two dopants, and overlapping is observed between the Ni 3d and B 2p states due to the bond formed between Ni and B. Also, the Ni 3d states are completely overlapped with the VBM, giving rise to bandgap narrowing of (2.49 eV); however, the B states appear deep in the bandgap region and separated by 1.10 eV from the CBM. Upon geometrical optimization of the Ni/BSub co-doped material, the local magnetic moment over the Ni ion becomes 0.843 μB; however, the magnetic moment over the whole lattice is 1.02 μB. In the Ni/Bint+sub co-doped system, an interaction exists between Ni and boron at the VBM and the total magnetic moment is 1.886 μB, while the local magnetic moment on Ni ion is 1.182 μB. Herein, the Ni 3d states are still overlapped with the VBM; however, most of the B states are found deep in the bandgap (Fig. 3b). Moreover, there are states with shallow character, corresponding to the formation of Ti3+. Due to these impurity states, many transitions can be observed upon visible light illumination and the charge carrier separation can be enhanced by the existing shallow states, in addition to the red shift in the calculated main bandgap (2.78 eV).
In the Se/Bsub co-doped anatase lattice, the PDOS and DOS is illustrated in Fig. 3c. The Se-occupied states can be observed at about 0.91 eV above the VBM, which overlap with the B states due to Se–B bond formation, while a separated B state is introduced in the bandgap at about 1.23 eV from CBM, indicating the allowed electron transitions on visible light irradiation. Moreover, the band gap is narrowed to 2.98 eV with a total magnetic moment of 0.67 μB for the whole system. The deep B states provide centers from which electrons can be excited on light absorption. Therefore, the charge carrier population increases; however, they may act as recombination centers for these carriers. Thus, the photocatalytic activity of Se4+/B is enhanced by the response to visible light, although the lifetime of the photo-produced carriers may be affected. Se/Bint+sub displays different electronic structures, and its calculated DOS and PDOS are illustrated in Fig. 3d. Similar to Ni/Bint+sub, the interaction between Se and B increases upon the incorporation of interstitial B. Moreover, the deep states due to substitutional B observed on Se/Bsub co-doping are placed in the forbidden gap at about 1.41 eV from the CBM on Se/Bint+sub co-doping. In addition, a shallow Ti3+ state appears, which is overlapped with the CBM. The calculated DOS analysis indicates that the bandgap is slightly blue shifted (3.31 eV); however, the visible light response can be enhanced by the transitions from the previously mentioned bandgap states. In addition, the shallow state can prolong the lifetime of the carriers. Thus, Se/Bint+sub-modified anatase TiO2 can be suggested as an enhanced photocatalyst.
Upon Ni/Se2− co-doping, the calculated bandgap is about 3.11 eV with the impurity states overlapping with the VBM in addition to the bandgap states separated by about 1.55 eV from the CBM. The PDOS with this co-doping shows a higher contribution of Ni 3d and Se states to the VB, as shown in Fig. 3e. According to the DOS calculations, it can be confirmed that the Se states are overlapped with the top of the VB, and the deep states exited in the bandgap are mainly due to the Se 4p states. Therefore, the Se2−, states which are either overlapped with Ni or isolated at about 1.56 eV from the VBM in Ni/Se2−, are due to the contribution of the Se 4p states. In the second case, Ni/Se4+ is co-doped as dual metal doping by the substitution of two close Ti ions. According to the DOS and PDOS shown in Fig. 3f, a state is observed at 2.50 eV from the CBM, indicating that more carriers are generated on visible light absorption. The calculated band gap is about 2.87 eV, which is higher than the case of Ni/Se2− co-doping, but still lower than pure TiO2, revealing a better response to visible light. For both materials (Ni/Se4+ and Ni/Se2−), the photocatalytic activity under visible light is improved due to the bandgap reduction and higher number of photogenerated carriers, but the deep states may affect the stability of the photogenerated carriers.
Ef = Edoped − Eundoped − (nMμM + nN−MμN−M) + (nOμO + nTiμTi) | (1) |
The lower the formation energy of defects, the more likely they are formed. Under O-rich conditions, the formation energy of metal mono-doping is lower than that of non-metal mono-doping. On the other hand, Se2− or B doping shows higher stability under Ti-rich conditions. Under both conditions, the formation energy is higher for Bsub than Bint and Bint+sub, which can verify the previously mentioned discussion of the metastable character of substitutional boron.22,33 The Bint+sub defect formation energy is the lowest value (−3.568 eV), suggesting that B at high concentration tends to occupy both the interstitial and substitutional sites.
The calculated formation energy for the co-doped defects demonstrates that defect co-doping is more facilitated under O-rich than Ti-rich conditions. However, the values for all the systems are more positive than the mono-doped cases except for Ni/Se4+, which exhibits a higher negative formation energy than Ni or Se4+ mono-doping. Moreover, Ni/Bsub, Ni/Bint+sub and Ni/Se2− co-doping and Bint mono-doping show the same value of formation energy under both conditions, indicating the independence of formation from the growth conditions.
(2) |
The UV-Vis optical absorption spectrum of anatase TiO2 is illustrated in Fig. 4a. The calculated bandgap for pristine anatase TiO2 is about 3.26 eV, which is about 0.06 eV higher compared to the experimental value.33 Therefore, all the anatase TiO2-based applications are limited to UV light, which contributes about ∼5% to solar irradiation. The spectra of the mono-doped and co-doped materials over pure anatase TiO2 are depicted in Fig. 4a and b, respectively. For all the materials, the absorption edge is red shifted considering the reference spectrum of pure TiO2 except for the Bint-doped materials. For the Ni mono-doped system, the light response extends up to about 2.5 eV, whereas the absorption edges are red shifted to about 1.6 and 2.2 eV for Se2− and Se4+ mono-doping, respectively. In B mono-doping, three different spectra for the three configurations Bsub, Bint and Bint+sub are observed. For Bsub, the absorption edge is red shifted to about 1.04 eV with a high absorption coefficient in the visible light region besides the absorption due to the main bandgap transition shown at about 3.18 eV. Bint and Bint+sub show different trends, where the absorption edge for both is blue shifted with absorption coefficients in the IR region, which are consistent with the states observed below the CB in the DOS.
Fig. 4 Calculated absorption coefficients with HSE hybrid functional for (a) mono-doped, and (b) co-doped anatase TiO2 materials. |
Upon co-doping, all the co-doped materials show an extended visible light response, indicating improved photoactivity over mono-doped materials. Ni/Bint+sub co-doping exhibits high absorption efficiency, indicating a high population of photogenerated charge carriers in addition to the red-shifted absorption due to the main bandgap excitations. Moreover, intense peaks are detected in the IR region, which confirm the transition from the shallow states located directly below the CB. The main absorption peak for Ni/Bsub co-doping is formed at about 2.5 eV. In addition, several peaks appear in the visible light region of the spectrum, but with a higher absorption coefficient than that of Ni/Bint+sub. Upon Se/Bsub co-doping, several absorptions can be observed in the visible light region with no absorption in the IR region as a result of the transitions from the deep states to the CB. Se/Bint+sub co-doping also shows visible light absorption, but with higher absorption coefficients than that of Se/Bsub co-doping. Additionally, a high intensity peak appears in the IR region, confirming the shallow state electron excitation expected from the DOS results. For Ni/Se co-doped anatase, the absorption corresponding to the bandgap excitations is red shifted to visible light for both the Ni/Se4+ and Ni/Se2− co-doped materials with energy values of about 2.9 and 3.1 eV, respectively. In addition, various peaks are shown for Ni/Se2− as a result of the electron transitions from the forbidden gap states to the CB.
Consequently, the visible light response is enhanced for all the materials except Bint-modified anatase. However, the absorption efficiency is better for the Se4+ mono-doped and Ni/Bsub and Se/Bint+sub co-doped systems, revealing the strength of these materials as effective photocatalysts under visible light.
Accordingly, the photocatalytic activity of the modified anatase TiO2 was evaluated for water splitting as an application for H2 production. The values of the VBE and CBE positions of pure anatase were calculated with respect to the normal hydrogen electrode (NHE) potential.5,6,51 For the doped system, the positions of edges of the valence and conduction bands were detected from the DOS analysis depending on their relative positions compared to pure anatase TiO2.10 The calculations for pure anatase TiO2 shows that the VBE is located at 2.94 eV, while the CBE position is 0.32 eV more negative than the reduction potential of H+/H2, which agrees with the previous experimental values.51 As shown in Fig. 5, the CBE position of the Se2− mono-doped system is almost similar to that of TiO2, whereas the VBE is shifted up by about 1.39 eV over TiO2 (about 0.32 eV more positive than the O2/H2O potential). This reveals that the reduction ability of H+ is maintained for Se2− mono-doped TiO2 with an increased tendency to release oxygen. In contrast, the CBE positions for the Ni and Se4+ mono-doped and Ni/Se4+ co-doped systems are shifted up by about 0.02, 0.08, and 0.08 eV over TiO2, respectively indicating that the reduction ability of H+ remains possible. In addition, their VBE positions are about 0.96, 0.55 and 0.87 eV more positive than the oxidation potential of O2/H2O, respectively, revealing that the ability to release oxygen is strong. Therefore, all the modified anatase materials, as shown in Fig. 5, can be candidates for water splitting and hydrogen production except for the Bsub mono-doped and NiSe2− co-doped systems. In the case of Bsub and Ni/Se2−, the CBE is about 0.30 and 0.34 eV more negative than the reduction potential of H+/H2; however, the VBE is about 0.49 and 0.02 eV more negative than the oxidation potential of O2/H2O, respectively. This means that the reduction ability of H+ ions is improved for Bsub and remains possible for Ni/Se2−, while the VBE position is unsuitable for the oxygen evolution reaction.
Fig. 5 Calculated band positions of mono- and co-doped TiO2 anatase materials. The values are with respect to the NHE potential in (V). |
Footnote |
† Electronic supplementary information (ESI) available: Fractional coordinates of the lowest energy co-doped structures. See DOI: 10.1039/d0ra07781j |
This journal is © The Royal Society of Chemistry 2020 |