Ningxin
Jiang
a,
Arun
Ramanathan
a,
Ryan E.
Baumbach
b and
Henry S.
La Pierre
*ac
aSchool of Chemistry and Biochemistry, Georgia Institute of Technology, Atlanta, Georgia 30332, USA. E-mail: hsl@gatech.edu
bNational High Magnetic Field Laboratory, Tallahassee, Florida 32306, USA
cNuclear and Radiological Engineering Program, Georgia Institute of Technology, Atlanta, Georgia 30332, USA
First published on 1st October 2020
The ground-state of S = 1 kagome lattice antiferromagnets (KLAFs), in the presence of strong geometric frustration and the smallest integer spin, has the potential to host a range of non-trivial magnetic phases including a quantum spin liquid. The effect of local geometry and metal-ion electronic structure on the formation of these predicted phases remain unknown due to, in part, the lack of an ideal analyte. Herein, a kagome lattice compound, (CH3NH3)2NaV3F12 (1-V), featuring a single distinct V3+ (d2) site in the Rm space group, was synthesized hydrothermally. In this S = 1, d2 system, the trivalent vanadium ions are tetragonally compressed due to Jahn–Teller distortion. The interlayer methylammonium cations show static positional disorder with three possible orientations. The negative Curie–Weiss temperature and dominant antiferromagnetic interactions make 1-V a candidate to study S = 1 KLAF physics. The frequency-dependence of ac magnetic susceptibility and the heat capacity results suggest that 1-V has a spin glass ground state. This freezing of the spin dynamics may be due to competing exchange interactions, structural imperfection arising from the static disorder of the interlayer methylammonium cations or the presence of ‘defect’-like spins.
Several S = 1 kagome lattice compounds have been synthesized before, but few compounds are close to an ideal S = 1 KLAF. The vanadium jarosites, AV3(OH)6(SO4)2 with A = Na+, K+, Rb+, Tl+, and NH4+, have nearly perfect kagome lattices but have dominant ferromagnetic interactions.20 Compounds with kagome lattice and S = 1 spins also include BaNi3(OH)2(VO4)2 (ref. 21) and [C6N2H8][NH4]2[Ni3F6(SO4)2],22 which show features of both antiferromagnetic and ferromagnetic interactions. The Ni3V2O8 has S = 1 and a kagome-staircase lattice which deviates from a planar 2-D kagome structure.23 The KV3Ge2O9 has a perfect kagome lattice above 50 K and strong antiferromagnetic interactions between spins.24 Nonetheless, below 50 K, the structure of KV3Ge2O9 is orthorhombic, and the C-centered symmetry is broken.25 Structural phase transitions can also be observed in m-N-methylpyridinium α-nitronyl nitroxide·BF4·1/3(acetone), m-(MPYNN)·BF4·1/3(acetone), and Na2Ti3Cl8.26–28 The YCa3(VO)3(BO3)4 is an interesting S = 1 KLAF with a possible QSL state.29,30 The short interlayer distance (∼2.9 Å) in comparison to the distance between neighboring vanadium within layers (∼5.3 Å) and the weak ferromagnetic interactions deviate this compound from an ideal two-dimensional S = 1 KLAF analyte. As a result, there is no phase stable kagome lattice system with S = 1 ions that are antiferromagnetically coupled and does not present structural perturbations. Recently, a group of compounds, A2BV3F12, with dominantly antiferromagnetic interactions and a large distance between layers, have been reported.24,31 However, the kagome lattices in these materials are distorted. Herein, building on our synthesis of the S = 1/2 KLAF, (CH3NH3)2NaTi3F12 (1-Ti),32 the analogous compound (CH3NH3)2NaV3F12 (1-V), an S = 1 kagome lattice antiferromagnet, is reported.
The vanadium kagome layers are separated by methylammonium (MA+) cations and sodium cations (Fig. 1b). The distance between layers is 6.367(1) Å. Similar to 1-Ti, the MA+ cations are disordered, and an analogous disorder model was applied to the MA+ in 1-V (Fig. S4b†). The nitrogen atoms occupy three crystallographically equivalent sites with 1/3 atom occupancy for each site, which suggests that each MA+ cations have three possible orientations. The distances between the hydrogen atoms of the amine group and their neighboring fluorides range from 1.9267(14) Å to 2.4581(10) Å and indicate the formation of H–F hydrogen bonding interaction.36
The crystal structure of 1-V is very similar to that of 1-Ti. The structural features of these two compounds are listed in Table 1.32 The θmp, which is the angle between the C–N bond of MA+ (the MA+ is composed of C1 and one of the nitrogen sites with C–N bond length of 1.44(3) Å for 1-V and 1.42(2) Å for 1-Ti) and (001) crystal plane in two compounds is 20.9(6)° in 1-Ti and 23.8(6)° in 1-V (demonstrated in Fig. S5†). The difference between the θmp value in 1-Ti and 1-V suggests that the inclusion of an organic cation provides essential flexibility in the structure to accommodate different sized trivalent cations in the with the same connectivity. The change in the θmp (the MA+ tilting angle) reflects changes in the size of the hexagonal pocket as the trivalent cation is varied.
1-V | 1-Ti | |
---|---|---|
Space group | Rm | Rm |
a, b/Å | 7.5349(13) | 7.7046(2) |
c/Å | 19.100(3) | 18.9645(6) |
d axial:dequi | 0.9566(10) | 0.9386(5) |
∠M–F–M/° | 146.02(5) | 146.09(4) |
Nearest-neighboring metal center distance/Å | 3.7675(5) | 3.8523(1) |
Layer distance/Å | 6.367(1) | 6.3215(2) |
θ mp/° | 23.6(8) | 20.9(6) |
Several S = 1 kagome lattice compounds, such as Na2Ti3Cl8 (ref. 27) and KV3Ge2O9,25 undergo phase transitions from Rm to lower symmetries. The SCXRD data of 1-V were also collected at 100 K, and there is no change in the measured lattice symmetry between 300 K and 100 K (Table S2†).17 Additionally, no feature of first-order phase transition was observed either in the differential scanning calorimetry from 183 K to 473 K (Fig. S9†) or in the heat capacity measurement from 2 K to 140 K at 0 T (Fig. 2d) which indicates that the Rm space group is maintained down to 2 K. The lack of phase transition and the absence of diffuse scattering in the precession image of (0kl) plane at 300 K and 100 K (Fig. S3†) indicates that the disorder of MA+ cations is static.32
The dc magnetic susceptibility measurement of 1-V was performed from 1.8 K to 300 K under field cooled (FC) and zero field cooled (ZFC) conditions under 0.001 T (Fig. 2a). Fits of the susceptibility data from 150 K to 300 K to the modified Curie–Weiss law with a temperature-independent contribution (see ESI† for details) yield a Curie–Weiss temperature of θcw = −39(3) K. This result suggests that the dominant interactions between spins are antiferromagnetic. The θcw is similar to the value of these A2BV3F12-type KLAFs with lattice distortion (Table 2).31 The effective magnetic moment of μeff = 2.361(23) μB/V3+ deviates from the theoretical value of 2.83 μB for S = 1 spin but is close to the value observed for several A2BV3F12 compounds.31,37 A change in slope around 8 K in the temperature-dependence of inverse susceptibility can be observed. This change in slope could be due to several effects including the formation of short-range magnetic ordering or the single-ion anisotropy of V3+ in the tetragonal environment. The strong single-ion anisotropy in the V3+, d2, cations has been observed in several systems such as in the alum doped with vanadium(III) cations and in the vanadium fluorides.20,31,38
Compounds | Space group | D M–M (Å) | Layer distance (Å) | θ cw (K) | T c (K) | Frustration parameterc | Description of the compound | Ref. |
---|---|---|---|---|---|---|---|---|
a D M–M indicates the distance between the nearest-neighboring metal (S = 1) centers. b T c represents any cooperative-ordering transition temperature. c Frustration parameter f = −θcw/Tc. The frustration parameters of compounds with dominant ferromagnetic interactions are not shown here since the frustration parameter is an empirical measure of frustration and applied mainly to antiferromagnetic systems.1 d In m-(MPYNN)·BF4·1/3(acetone), the S = 1 spin is composed of two ferromagnetically coupled spins, the distance between spins is therefore hard to determine. e The antiferromagnetic coupling constant, J1, between S = 1 spins is −3.1 K. | ||||||||
1-V | Rm | 3.7675(5) | 6.367(1) | −39(3) | 2.3 | 16.2 | 2D kagome lattice with one distinct V3+ site, antiferromagnet | This work |
Rb2NaV3F12 | P21/m | 3.680–3.709 | 6.168 | −50 (H⊥ab) | 8.0 | 6.25 | Distorted 2D kagome lattice, antiferromagnet | 31 |
Cs2NaV3F12 | P21/m | 3.707–3.732 | −21 (H⊥ab) | 4.9 | 4.28 | Distorted 2D kagome lattice, antiferromagnet | 31 | |
Cs2KV3F12 | P21/c | 3.734–3.743 | −29 (H⊥ab) | 2.5 | 11.6 | Distorted 2D kagome lattice, antiferromagnet | 31 | |
NaV3(OH)6(SO4)2 | Rm | 3.642, 3.643 | 5.617 | +53 | 33 | N.A. | Nearly perfect kagome lattice, ferromagnet | 20 and 44 |
MV3(OH)6(SO4)2, M = Na+, K+, Rb+, Tl+ and NH4+ | Rm | 3.636–3.642 | 5.800–5.973 | 52–54 | 29–31 | N.A. | Nearly perfect kagome lattice, ferromagnet | 20 and 45 |
BaNi3(OH)2(VO4)2 | C2/c | 2.908, 2.938 | 7.028 | 10 | 15 | N.A. | Distorted kagome lattice, both ferromagnetic and antiferromagnetic | 21 |
[C6N2H8][NH4]2[Ni3F6(SO4)2] | R | 3.658 | 8.731 | −60 | 10 | 6 | Perfect kagome lattice, both ferromagnetic and antiferromagnetic | 22 and 46 |
(NH4)2(C2H8N)[V3F12] | P21/m | 3.711, 3.722 | 6.932 | −30 | 15 | 2 | Distorted kagome lattice, both ferromagnetic and antiferromagnetic | 37 |
KV3Ge2O9 | P63/mmc (above 50 K) | 2.931 | 6.855 | −250 | ∼60 (structural phase transition | ∼4.2 | Perfect kagome lattice at high temperature, orthorhombic phase below 50 K, antiferromagnet | 24 and 25 |
YCa3(VO)3(BO3)4 | P | 5.244–5.262 | 2.898 | −453 | <1.5 | >302 | Distorted kagome lattice, antiferromagnet, short interlayer distance, QSL candidate | 29 and 30 |
m-MPYNN)·BF4·1/3(acetone) | P3c1 (above 129 K) | N.A.d | 11.81 | N.A.e | 128.7 (structural phase transition) | N.A. | Kagome lattice antiferromagnet | |
Ni3V2O8 | Cmca | 2.942, 2.968 | 5.710 | −30 | 2.6, 4, 6.4, 9 | <11.6 | Kagome-staircase lattice, antiferromagnet | 23 |
Strong interlayer or intralayer ferromagnetic interactions have been observed in several S = 1 kagome lattice compounds (Table 2). The negative θcw (inset of Fig. 2a) indicates that 1-V has dominantly antiferromagnetic interactions, which is similar to the other A2BV3F12 compounds.31,37 Therefore, the 1-V, with a non-distorted kagome lattice and dominantly antiferromagnetic interactions is a candidate material to study the ground state of S = 1 KLAFs. The frustration parameter f = |θcw/Tc| (Tc represents any cooperative-ordering transition temperature) is an empirical measurement of frustration.1 The f in 1-V is 16.2, which indicates strong frustration and is larger than the value for the previously reported S = 1 KLAFs except for the YCa3(VO)3(BO3)4 (ref. 29) (Table 2).
The FC and ZFC susceptibility curves under 0.001 T increase monotonically with decreasing temperature until 2.4 K where a peak is found in the ZFC curve. This peak can be observed from 0.005 T to 0.1 T, and the position of the peak does not change as a function of applied field (Fig. S10†). The divergence between FC and ZFC curves from 1.8 K to 8 K as shown in the inset of Fig. 2a suggests the freezing of spins at low temperatures. The spin freezing behavior is supported by the frequency dependence of the real part of the ac susceptibility, χ′ (Fig. 2c), and the sudden onset of the imaginary part of the ac susceptibility, χ′′, (Fig. S12†) from 1.8 K to 5 K under 0 T.39 Additionally, a maximum that shifts to higher temperatures with increasing frequency can also be observed around 3 K. The empirical parameter X, which is used to express the freezing temperature observed in χ′ vs. frequency dependence, is around 0.06 in 1-V and is within the range for insulating spin glasses.40 A broad peak centers at 4.4 K is found in the temperature dependence of specific heat under 0 T, and this broad peak shifts to 4.9 K and reduces in intensity under 9 T (Fig. 2d). A typical spin glass shows a peak in both dc and ac magnetic susceptibility, a divergence between FC and ZFC dc magnetic susceptibility curves, a frequency dependence of the χ′, and a sudden onset of χ′′ near spin glass transition temperature (Tf).39 The heat capacity of a spin glass shows a broad peak at a temperature higher than the Tf.39 Therefore, the physical properties of 1-V are consistent with those of a spin glass.
In an ageing experiment, a spin glass presents a divergent response to the application of applied field which implies nonequilibrium dynamics.41–43 On 1-V, an ageing experiment was performed by cooling the sample under zero field from 50 K (above the Tf in 1-V) to the measurement temperature (Tm). At Tm, the sample was aged for the waiting time, tw, seconds. Then, a small magnetic field (0.0025 T) was applied and the magnetization as a function of time was recorded. The results are shown in Fig. 3. The magnetic moment as function of time shows a clear dependence on tw. This dependence is observed only at 1.8 K (not at 3.0 K or 5.0 K) which is consistent with a spin glass behavior below Tf for 1-V.43 The time dependence of magnetization at 1.8 K can be fit by the stretched exponential function as shown in Fig. S15†.47 The increase of time constant τ with longer tw is indicative of a stiffening of the spin relaxation.47 An inflection point is absent in the first derivative of the time dependence of magnetization as shown in Fig. 3b. However, an inflection point can be observed close to the tw for a typical metallic spin glass, such as CuMn.42 The ageing behavior of 1-V is close to the behavior in La0.5Sr0.5CoO3 which can be described as a cluster glass or mictomagnet (one category of spin glass) due to the formation of large magnetic clusters.48
The isothermal magnetization of 1-V at 1.8 K is shown in Fig. 2b. No hysteresis is observed in the magnetization curves of 1-V between −1 T and 1 T (inset of Fig. 2b). A high-resolution of isothermal magnetization measurement was conducted in a short loop as shown in Fig. S16† and an observable hysteresis is noted. While this is a small hysteresis, it is consistent with the assignment of the 1-V as a spin glass. The magnetization under 14 T is 0.383 μB/V3+ which is around 19% of the saturated value for V3+ ions (2 μB/V3+ when g = 2). The magnetization increases rapidly below 10 T and is linearly dependent on the field above 10 T. The magnetization is far from saturation at accessible fields and is indicative the significant geometric frustration and the strong antiferromagnetic interaction.
One possible way to analyze the isothermal magnetization result is that the magnetization could be consisted of two components, the defect (Md) and the intrinsic (Mi) contributions, which is a similar approach to that utilized for 1-Ti. After the subtraction of the linear dependent component (Mi, red dashed line in Fig. 2b, this component is determined by the linear fitting of the isothermal magnetization data above 10 T), around 3% of ‘defect’-like S = 1 spins (Md) could be identified as shown in the orange dots in Fig. 2b. These ‘defect’-like spins saturate rapidly below 10 T, but still deviate from the Brillouin function for 2.84(3)% of free S = 1 spins (green dashed line in Fig. 2b). However, the XPS results have largely ruled out the existence of vanadium species with different oxidation states in 1-V and no impurity phases can be observed in laboratory PXRD. Therefore, the origin of the non-linear region in isothermal magnetization result at low field still requires further structural, spectroscopic, and physical studies.
The 1-V and 1-Ti are structurally similar (Table 1) and share some similar physical properties (Table S3†). Both compounds have dominant antiferromagnetic interactions and are highly frustrated. Frequency dependence can be observed in the real part of ac magnetic susceptibility in both 1-V and 1-Ti, while a peak can only be found in 1-V around 3 K. Evidence of ‘defect’-like spins can be observed in both compounds and no chemical impurities are identified by laboratory PXRD in either material.
It should be noted that recent theoretical studies propose that the introduction of structural disorder in KLAFs could lead to a spin glass state.49,50 It is possible that the magnetic freezing behaviors observed in both compounds are induced by the disordered methylammonium cations. It is also noticeable that θcw in 1-V is higher than that in 1-Ti (−36 K vs. −140 K) which implies stronger antiferromagnetic interactions between spins in 1-Ti than in its isostructural 1-V. The weaker antiferromagnetic coupling in 1-V could originate from additional, competing, ferromagnetic exchange interaction due to the extra d electron in either dxz or dyz orbitals for V3+ in comparison to Ti3+.37 Similar phenomenon has been observed in the jarosites with V3+, Cr3+ and Fe3+.4,20 Therefore, we cannot rule out the contribution from the potential competing ferromagnetic exchange interaction to the spin glass state in 1-V despite of the dominant antiferromagnetic interactions between spins. In addition, the ‘defect’-like spins could also lead to the spin glass state since several spin glasses are induced by the inclusion of intrinsic ‘impurities’ such as the metallic alloy CuMn with 0.9% Mn.40
Footnote |
† Electronic supplementary information (ESI) available: Synthetic, spectroscopic, and crystallographic details (PDF and CIF). CCDC 1987388 and 1987389. For ESI and crystallographic data in CIF or other electronic format see DOI: 10.1039/d0sc03323e |
This journal is © The Royal Society of Chemistry 2020 |