Nicolai D.
Knöfel
a,
Hannah
Rothfuss
b,
Pavleta
Tzvetkova
d,
Bragavie
Kulendran
a,
Christopher
Barner-Kowollik
*bc and
Peter W.
Roesky
*a
aInstitute of Inorganic Chemistry, Karlsruhe Institute of Technology (KIT), Engesserstrasse 15, 76131 Karlsruhe, Germany. E-mail: roesky@kit.edu
bMacromolecular Architectures, Institute for Chemical Technology and Polymer Chemistry, Karlsruhe Institute of Technology (KIT), Engesserstrasse 18, 76131 Karlsruhe, Germany. E-mail: christopher.barner-kowollik@kit.edu
cCentre for Materials Science, School of Chemistry and Physics, Queensland University of Technology (QUT), 2 George Street, Brisbane, Queensland 4000, Australia. E-mail: christopher.barnerkowollik@qut.edu.au
dInstitute of Organic Chemistry, Institute for Biological Interfaces 4 – Magnetic Resonance, Karlsruhe Institute of Technology (KIT), Fritz-Haber-Weg 6, 76131 Karlsruhe, Germany
First published on 24th August 2020
We introduce the formation and characterization of heterometallic single-chain nanoparticles entailing both catalytic and luminescent properties. A terpolymer containing two divergent ligand moieties, phosphines and phosphine oxides, is synthesized and intramolecularly folded into nanoparticles via a selective metal complexation of Pt(II) and Eu(III). The formation of heterometallic Eu(III)/Pt(II) nanoparticles is evidenced by size exclusion chromatography, multinuclear NMR (1H, 31P{1H}, 19F, 195Pt) as well as diffusion-ordered NMR and IR spectroscopy. Critically, we demonstrate the activity of the SCNPs as a homogeneous and luminescent catalytic system in the amination reaction of allyl alcohol.
As a rare example, Lemcoff and colleagues designed heterobimetallic single-chain nanoparticles via the introduction of catalytically active Ir(I) and Rh(I) ions into a diene-functionalized polymer chain.11 However, no targeted metal placement was carried out, as merely one type of ligand moiety was present, suitable for both metal species. Thus, the introduction of orthogonal linker moieties into the polymer chain is mandatory for a selective and controlled incorporation of different metal ions. To form heterometallic SCNP structures, at least one of the metal precursors needs to induce the chain collapse, whereas a second metal species coordinating to an orthogonal ligand system can add additional functionality. Striving for a SCNP system, which exhibits both luminescent and catalytic properties, we herein report the synthesis and in-depth characterization of a bifunctional terpolymer, featuring both phosphine and phosphine oxide ligand moieties. The terpolymer enables SCNP formation via orthogonal complexation of platinum(II) and europium(III), providing novel catalytic material (Fig. 1). The combinatorial design of catalytic and luminescent properties within a SCNPs system allows i.e. the visualization and tracking of the polymer nanoparticles during catalysis and helps to monitor a successful catalyst separation.
Scheme 1 Synthesis of bifunctional terpolymer PP/Oxidevia nitroxide mediated polymerization of styrene, 4-(diphenylphosphino)styrene and 4-(diphenylphosphino oxide)styrene. |
Analysis resulted in a monomer ratio of approx. 3.5 mol% phosphine and 1.7 mol% phosphine oxide functionalities in the terpolymer, in agreement with the feed ratio. The given values are – within the margin of error of NMR spectroscopy – estimates which are additionally hampered by the solvent resonance in the 1H NMR spectrum. Therefore, 31P{1H} NMR experiments, applying bis(diphenyl-phosphino)methane (DPPM) as an external standard, were additionally performed and resulted in 0.17 mmol phosphine oxide and 0.35 mmol phosphine species per 1 g of terpolymer PP/Oxide (Fig. S21†), which is in agreement with the priorly determined values. Accordingly, two resonances, in a ratio of 2:1, are observed at δ = −6.2 ppm and δ = 29.2 ppm in the 31P{1H} NMR spectrum of PP/Oxide, attributed to the implemented triarylphosphine and triarylphosphine oxide species (Fig. 4A). The characterization of PP/Oxidevia SEC (THF, RI) resulted in Mp = 41 400 g mol−1 (average molecular weight 25300 g mol−1 ) with a dispersity of Đ = 1.4 (Fig. 3, top). Combining the results of the SEC and NMR analysis, approx. 8–9 phosphine and 4 phosphine oxide moieties are estimated per chain. In addition, PP/Oxide was analyzed by IR spectroscopy (ESI, Fig. S22†). Among others, characteristic bands at = 1202 and = 1118 cm−1 are attributed to the PO vibrational stretching and C–H deformation mode of the triarylphosphine oxide units.23,24
Herein, cod is readily substituted by two phosphine ligands of PP/Oxide, as already established in previous studies on Pt(II)-linked SCNPs.8 The orthogonal properties of the phosphine oxide ligands, which do not coordinate to Pt(II), allow for the simultaneous complexation of a second suitable metal species. Thus, the europium precursor [Eu(dbm)3(H2O)2] (dbm = dibenzoyl-methanide) was employed, coordinating exclusively to the phosphine oxides, via release of H2O, yielding Eu(dbm)(III)/Pt(II)–SCNPs. Hereby, the phosphine oxide Eu(III) coordination can be realized either prior or subsequent to the Pt induced chain folding, resulting in an analogue Eu(III)–Pt(II)–SCNP system. Thus, the nanoparticle formation is independent from the sequence of metal ion addition, allowing dual functionalization and single-chain collapse in one step. Additional experiments, investigating stepwise metal addition and selective coordination behavior of platinum and europium towards the disparate ligand systems, are presented in the ESI (Schemes S4 and S5†). In theory, the attachment of either one or two phosphine oxides to a [Eu(β-diketonate)3] species is possible.25,26 However, the small number of approx. four phosphine oxide units per chain, combined with a high steric demand of the rigid polymer backbone suggests a 1:1 coordination ratio. In addition, the coordination of [Eu(dbm)3] to a sole triarylphosphine oxide functionalized copolymer (styrene based) was investigated at high concentrations. Yet, no network formation was observed, as it is expected in case of a 2:1 ligand to Eu(III) coordination. For this reason, an Eu(III) coordination ratio of 1:1 is presumed. This assumption was further confirmed by DOSY NMR measurements (see below).
Following an analogous reaction procedure, different Eu(III) complexes can be applied, emphasizing the versatile applicability of the bifunctional polymer system. In case of the precursor [Eu(tta)3(H2O)] (tta = thenoyltrifluoroacetonate) heterometallic Eu(tta)(III)/Pt(II)–SCNPs were obtained, exhibiting e.g. a convenient 19F NMR sensor (Fig. 2 and ESI, Scheme S3†).
Fig. 2 19F NMR spectrum of Eu(tta)(III)/Pt(II)–SCNPs in CDCl3. The tta moiety of the Eu(III) moiety allows tracking of the SCNPs in solution via19F NMR spectroscopy. |
To confirm the assumption of an orthogonal metal complexation and verify the metal-induced chain compaction, the obtained particles were thoroughly investigated (for detailed analysis of the Eu(tta)(III)/Pt(II)–SCNPs refer to ESI†). The expected collapse into a more compact structure was verified by SEC analysis (THF, RI).27 In comparison to the terpolymer PP/Oxide, the SEC trace for the Eu(dbm)(III)/Pt(II)–SCNPs is shifted towards longer retention times (Fig. 3, top), indicating a smaller hydrodynamic radius and thus pointing to the formation of nanoparticles without intermolecular side reactions. Further, the curve indicates the existence of a small molecular species (not shown in the spectrum), which most likely originates from unbound europium(III) complexes. To some extent the phosphine oxide coordination is apparently not sufficiently strong to withstand SEC measurement conditions. Consequently, the depicted SEC elugram rather represents a trace of Pt(II)-linked SCNPs. Furthermore, the transition of the linear terpolymer into a more compact nanoparticle was demonstrated by diffusion ordered spectroscopy (DOSY).28,29 Based on the obtained diffusion coefficients, the hydrodynamic radii of the particles were calculated, applying the Stokes–Einstein equation (see ESI†). The mean hydrodynamic radius of PP/Oxide resulted in rH = 8.0 nm, whereas a radius of rH = 1.9 nm was determined for the Eu(dbm)(III)/Pt(II)–SCNPs. Interestingly, sole addition of [Eu(dbm)3(H2O)2] to PP/Oxide, resulting in the intermediate metallopolymer ‘PP/Oxide–Eu(dbm)3’, affording a slightly larger hydrodynamic radius of rH = 11.2 nm. Hence, the addition of an Eu species to PP/Oxide does not seem to induce chain compaction. The results are in line with a 1:1 coordination ratio of Eu(III) to the phosphine oxide ligands of PP/Oxide, confirming the orthogonal behavior of the two ligand moieties.
To determine the photophysical properties, photoluminescent emission (PL) spectra of the Eu(dbm)(III)/Pt(II)–SCNPs were recorded in the solid state (Fig. 3, bottom). After excitation at λ = 350 nm, the spectrum features characteristic bands resulting from 4f–4f transitions (5D0–7FJ) and is dominated by a band at λ = 612 nm (5D0–7F2 transition).25,30 The resulting bright red luminescence is typical for europium(III) compounds.17,31 The coordination of phosphine oxide moieties to Eu(III)-diketonates is reported to further enhance the luminescence, working as an antenna ligand.21,25 As 4f–4f transitions are virtually unaffected by the surrounding ligands of Eu(III), an almost identical emission spectrum is observed for the Eu(tta)(III)/Pt(II)–SCNPs (see ESI, Fig. S26†). However, the non-symmetric tta moiety of the Eu(III) species results in a visibly more intense luminescent behavior of the corresponding nanoparticles.
Furthermore, the Eu(dbm)(III)/Pt(II)–SCNPs were characterized by multinuclear NMR spectroscopy, primarily to gain closer insights into the metal coordinated folding units. In the 31P{1H} NMR spectrum (CDCl3) of the SCNPs, the resonance of the triarylphosphines at δ = −6.2 ppm (Fig. 4A) is not detected anymore. Instead, an intense resonance at δ = 13.5 ppm is observed, accompanied by platinum(II) satellites (d, 1JP,Pt = 3661 Hz), which are attributed to square planar cis-[PtCl2(PPh2Ar)2] folding units (Fig. 4B).
A minor resonance at δ = 19.5 ppm is assigned to the corresponding trans-species. The obtained data are in agreement with isostructural Pt(II)–SCNPs and analogous model complexes.8,32 The high preference for a cis-geometry of the Pt(II) centers, approx. 30:1 (cis/trans), is rationalized by the predetermined arrangement of the precursor complex cis-[PtCl2(cod)] as well as the steric constraints of the polymer backbone. Furthermore, the resonance at δ = 29.1 ppm, corresponding to the phosphine oxide moieties, is still present. However, in comparison to PP/Oxide, the resonance is broadened, resulting in a decrease in its integral value. This is presumably caused by the coordination to the paramagnetic europium(III) cores.33 This effect is also observed in the alike 31P{1H} NMR spectrum of the Eu(tta)(III)/Pt(II)–SCNPs (ESI, Fig. S8†). In the 195Pt NMR spectrum of the Eu(dbm)(III)/Pt(II)–SCNPs, a triplet resonance for the cis-[PtCl2(PPh2Ar)2] folding units is detected at δ = −4420 ppm (t, 1JPt,P = 3715 Hz), confirming the obtained 31P{1H} NMR data (ESI, Fig. S6†). The coordination of [Eu(dbm)3] to the phosphine oxide moieties of PP/Oxide is additionally evidenced by 1H NMR spectroscopy. In the corresponding spectrum a characteristic high field resonance at δ = 16.9 ppm is attributed to the methine group of the dbm ligands (ESI, Fig. S4†). Further information was obtained by IR spectroscopy. In the IR spectrum of the Eu(dbm)(III)/Pt(II)–SCNPs bands for the dbm ligands are detected at = 1519 cm−1, 1549 cm−1 and 1600 cm−1 (ESI, Fig. S23†), pointing towards its successful encapsulation in PP/Oxide.
The results are similar to the data obtained for the literature-known Pt(II)–SCNPs as well as the monomeric platinum complex cis-[Pt(PPh3)2Cl2], yet a different reaction procedure and catalyst loading need to be considered when compared in detail.8 After the catalytic reaction, the SCNPs were readily isolated by precipitation in methanol, or subsequent column chromatography (e.g. acetone, neural aluminum oxide). In the latter case, they remained on top of the column and were readily detected when irradiated with UV light (Fig. 5, applying Eu(tta)(III)/Pt(II)–SCNPs as catalyst). Thus, for this specific reaction a simple detection mode for the catalyst's separation was achieved. UV illumination of the filtrate after column chromatography showed no luminescence, thus indicating a complete catalyst separation. However, the photoluminescence of the catalyst is visibly reduced during catalysis, most likely due to the formation of H2O and thermal decomposition, leading to partial quenching of the Eu(III) species over time (ESI, Fig. S33†). Thus, recycling of the catalyst, as it has been previously studied for Pt(II)–SCNPs,8 was not further pursued, as the luminescence was significantly reduced in the second cycle. Additionally, in case of the Eu(tta)(III)/Pt(II)–SCNPs19F NMR studies revealed that the diketonate ligands of the Eu(III) complex are partially removed with increasing reaction temperature and time. Additionally, in the eluant of the chromatography a weak resonance in the 19F NMR spectrum is detected, attributed to unbound tta ligands, confirming partial decomposition during catalysis.
Advantageously, the amount of phosphine and phosphine oxide moieties can readily be adjusted. Thus, for future studies, an introduction of task-specific quantities of Pt(II) and Eu(III) centers, as well as the implementation of other metal combinations, is feasible.
Footnote |
† Electronic supplementary information (ESI) available: NMR- and IR-spectra. See DOI: 10.1039/d0sc03579c |