Pawin
Iamprasertkun
*ab,
Wisit
Hirunpinyopas
c,
Varisara
Deerattrakul
d,
Montree
Sawangphruk
b and
Chakrit
Nualchimplee
a
aDepartment of Applied Physics, Faculty of Sciences and Liberal Arts, Rajamangala University of Technology Isan, Nakhon Ratchasima, 30000, Thailand. E-mail: pawin.ia@rmuti.ac.th
bDepartment of Chemical and Biomolecular Engineering, School of Energy Science and Engineering, Centre of Excellence for Energy Storage Technology (CEST), Vidyasirimedhi Institute of Science and Technology, Rayong, 21210, Thailand
cDepartment of Chemistry, Faculty of Science, Kasetsart University, Bangkok 10900, Thailand
dDepartment of Chemical Engineering, Faculty of Engineering, Kasetsart University, Bangkok 10900, Thailand
First published on 30th September 2020
A new approach using graphene as a conductive binder in electrical supercapacitors has recently been proposed. Graphene shows outstanding properties as a conductive binder, and can be used to replace conductive, additive, and polymer binders. However, graphene follows an EDLC behaviour, which may limit its electrochemical performance. In the process described in this work, we introduced WSe2 nanoflakes as a new approach to using pseudocapacitive materials as binders. The WSe2 nanoflakes were produced through liquid phase exfoliation of bulk WSe2, and the flake size was finely selected using a controlled centrifugation speed. The physical and electrochemical properties of the exfoliated WSe2 flakes were analysed; it was found that the smallest flakes (an average flake size of 106 nm) showed outstanding electrochemical properties, expanding our understanding of transition metal dichalcogenide (TMD) materials, and we were able to demonstrate the applicability of using WSe2 as a binder in supercapacitor electrodes. We also successfully replaced conductive additives and polymer binders with WSe2. The overall performance was improved: capacitance was enhanced by 35%, charge transfer resistance reduced by 73%, and self-discharge potential improved by 9%. This study provides an alternative application of using TMD materials as pseudo capacitive binders, which should lead to the continued development of energy storage technology.
The role of a polymer binder such as polyvinylidene fluoride (PVDF) or polytetrafluoroethylene (PTFE) is to bind the materials with the current collector. However, these binders are electrical insulators made from non-capacitive materials, which suppress the overall device performance through poor capacitance and high electrical resistance.5 This means that a conductive additive such as carbon black must be used to minimise interfacial resistance.6 The polymer binder also blocks some of the pores in the active materials, reducing the overall surface area.7 This is a critical issue in the development of large scale energy storage devices.
A new approach to address this issue has been proposed recently by the Bin Xu and Yury Gogotsi,7,8 which used reduced graphene oxide (rGO) as a multi-functional conductive binder for fabricating flexible and free-standing carbonaceous electrodes. This strategy has been further expanded to the manufacture of batteries9–11 and hybrid capacitor electrodes12 using other two-dimensional (2D) materials such as MXene.13
However, graphene stores the charge through a build-up in the electrical double layer, which can limit the energy density of the energy storage.4,14,15 There are many 2D materials apart from graphene that can be used, such as transition metal dichalcogenides (TMDs, also called MX2),16 which provide outstanding electrochemical properties in terms of energy storage.17 This is due to the charge storage mechanism of these materials based on both faradaic and non-faradaic processes.18 This means that we have the opportunity to replace the graphene conductive binders with TMD materials in this context.
Herein, we have introduced WSe2 nanoflakes as alternative binder materials to produce a new type of electrode based on the concepts of pseudocapacitive binder. In this experiment, the WSe2 nanoflakes were produced through the liquid phase exfoliation of bulk WSe2. The flake dimensions were finely tuned by controlling the centrifuge speed, as exfoliated WSe2 is produced in different sizes at different revolution speeds. To the best of our knowledge, there have been no prior studies on electrochemical properties based on size dependent WSe2 flakes and no attempts have been made to use these materials as pseudo capacitive binders. This work helps the development of electrode manufacturing and is designed to improve high performance energy storage devices.
According to Coleman et al., the flake sizes of TMD materials diminish with increasing centrifugation speeds;22 we therefore controlled the size of WSe2 flakes by centrifuging the supernatant at 3000, 6000, and 12000 rpm. The size controlled WSe2 flakes were collected from the sediment after each step (see Fig. 1a). The flake size distribution from the collected sediment is shown in Fig. 1b. Overall, it can be clearly seen that the major population of the flake size was found to be 106, 255, 205, 396, and 955 nm. The exfoliation yield from this technique is shown in Fig. 1c.
(1) |
γsv − γsl − γlvcosθ = 0 | (2) |
The electronic conductivities of the prepared electrodes were calculated from σ = L/RA where R was measured using the 2 probe method, and L and A are the thickness and the exposed area of the prepared electrodes.
The TEM image in Fig. 3 displays a similar flake size where the high centrifugation speed exhibits small flakes as well as low thickness. It is found that the centrifugal speed over 12000 rpm provides a lateral flake size between 20 nm and 100 nm (see Fig. 3a), confirming the results from DLS and SEM techniques. Moreover, the high resolution TEM images (gold colour box) clearly present mono- to few-layer WSe2 nanosheets, and the WSe2 atoms are arranged in the 2H phase as can be seen in the inset image. Then again the WSe2 flakes become larger and thicker when the centrifugal rate is reduced, which can be seen from Fig. 3b–e, respectively.
The Raman spectra shown in Fig. 4a show predominantly Raman features for each of the flake sizes. The Raman spectra of bulk WSe2 show two dominant peaks at approximately 249 cm−1 and 257 cm−1, which can be assigned to the E12g and A1g modes.29 It was found that after the exfoliation and separation processes, the intensity of the A1g peak diminished and shifted to a lower frequency, indicating fewer layers.30 For monolayer WSe2, there is no frequency difference between E12g and A1g peaks, and the two peaks share the same position.30 It is evident that higher centrifugal speeds provided a flake thickness from a single layer to few layers, as the E12g and A1g share the same position. Until the number of layers increases to four layers, there is no significant change in the Raman feature.31 To further confirm the thickness of the WSe2 flakes, the peak of 2θ – about 13.7° of the XRD pattern, referring to the (002) reflection plane of 2H-WSe2 – is shown in Fig. 4b. Note that the interlayer spacing of the bulk material is calculated at approximately 0.68 nm. After exfoliation, it can be clearly seen that the FWHM decreases in accordance with the increases of the WSe2 flakes representing the diminishing number of layers,19 which once again reflects similar results from the SEM, TEM, and Raman techniques. Moreover, it was found that the (002) plane shifted to a lower degree once the flake size became smaller, which reflects the increase of WSe2 layer spacing.32
In order to explain the surface chemical composition of the exfoliated materials, the XPS in Fig. 5a and b show the W 4f and Se 3d of 106 nm flakes (quoted as “>12.0k”), respectively. The XPS spectra under other centrifugal conditions are given in Fig. S1 and S2.† Overall, the 106 nm WSe2 flakes display four peaks, at 32.4 eV, 34.5 eV, 36.5 eV and 38.3 eV, which can be divided into two components: (1) W 4f7/2 and W 4f5/2 of W Se2, and (2) W 4f7/2 and W 4f5/2 of the W–O bond, also referring to (W6+) of tungsten as shown in Fig. 5a.33 This oxide form is likely to have been caused by the partial oxidation at the edge and a defective atom in the WSe2. This feature is typically observed in the TMD family.18 Apart from the tungsten element, the narrow spectra of Se 3d in Fig. 5b show two peaks at 54.6 eV and 55.4 eV, providing a peak separation of 0.8 eV, which agrees with the binding energy of WSe2 crystals.34 We further analysed the atomic concentration between WSe2 and WO3 in each of the flake sizes (see Fig. 5c), and found that the exfoliation process could be used to remove any surface oxide and provide a higher yield of WSe2 of up to 78% by atomic concentration for the 106 nm WSe2 flakes.
To explore the applicability of the WSe2 in the electrochemical context further, the electrochemical properties of each of the flake sizes were explored using CV and GCD in 0.5 M KCl as shown in Fig. 6. Overall, it was clear that all the WSe2 flake sizes exhibited a small vertex potential window of about 0.6 V (from 0.0 to −0.6 V vs. carbon) due to the catalytic properties of WSe2 for the hydrogen evolution reaction (HER)35 (see Fig. 6a). It was also noted that the CV in Fig. 6b of 106 nm flakes provides the highest specific current. The capacitance of 106 nm flakes is about 5.1 F g−1 at 10 mV s−1, and decreases to 1.7 F g−1 after increasing the scan rate to 100 mV s−1. These quoted capacitances are lower than those that have occasionally been reported for the TMD family, this is because there are no conductive additives or polymer binders added. So far, the mass of these additives is often excluded from the calculations.18 Meanwhile, it was found that the WSe2 flakes provide higher specific capacitance than those of previously reported TMD materials such as MoS2 (3.4 F g−1), WS2 (3.5 F g−1), and TiS2 (4.6 F g−1) under the same measurement conditions and electrode preparation procedures.32 This may therefore provide an opportunity for further development of WSe2 composite electrodes similar to MoS2. Apart from the outstanding electrochemical performance of the smallest WSe2 flakes (106 nm), there is a capacitance dependence on associated scan rates for all flake sizes, as can be seen in Fig. 6b. This is due to the limit of ionic diffusion to the WSe2 galleries,19 and it has been surmised that pseudocapacitive contributions are involved in evaluating the total capacitance. We therefore subsequently analysed the current through the surface and diffusion controlled processes according to eqn (3).36
i(V) = k1v + k2v1/2 | (3) |
(WSe2)surface + K+ + e− ↔ (WSe2−K+)surface | (4) |
WSe2 + K+ + e− ↔ WSe − SeK | (5) |
It is evident that the dimensions of smaller flakes provide a significantly higher pseudocapacitance than the dimensions of the larger flakes. One possible reason for this is that we successfully removed the oxide forming at the edge or defect sites of WSe2 leading to higher pseudocapacitive contributions from the WSe2 component. However, there is also a contribution from the physisorption process as shown in eqn (6).19 The diminished capacitance may also be due to the poor surface area of large WSe2 flakes.
WSe2 + K+ ↔ WSe − SeKads+ | (6) |
Note that the total capacitances, including physisorption (also known as EDLC), surface redox and ion intercalation as well as the coulombic efficiency for each flake size measured using the GCD technique, are given in Fig. 6d. This total capacitance agrees with the capacitance calculated using the CV technique.
To further confirm the charge storage mechanisms of the prepared electrode material, the EIS were then described according to the complex model of capacitance using eqn (7)–(9).37
C = C′ − jC′′ | (7) |
(8) |
(9) |
Overall, the Nyquist plots of all flake sizes in Fig. 7a show a straight line near the vertical axis indicating capacitor behaviour. However, it is noticeable that the internal resistance (Rs) relies on the flake dimensions, with the Rs becoming larger as the flake dimensions increase. This also explains why the capacitance of larger WSe2 flakes is smaller than those of the smallest flakes. Apart from the resistance, the normalised real part capacitance in Fig. 7b refers to the characteristic of the electrode/electrolyte interface.38 Evidently, the real part capacitance of all flake sizes decreases as the frequency increases in a similar pattern due to the identical characteristics of the electrode materials and the electrolyte. In contrast, the response across the frequency range from the imaginary part capacitance behaves the other way round for each of the flake sizes (see Fig. 7c). It is noticeable that the peak of about 1 Hz increases with the decrease in flake dimensions. This is due to the increase in the pseudocapacitive contribution (i.e. the ion intercalation) which confirms the calculations we arrived at in the previous section. Moreover, the Bode plot in Fig. 7d shows different phase angle responses across the applied frequency, referring to a diverse relaxation time constant value. It was found that the time constant decreased from 167 ms to 4.53 ms as the flake size was reduced.
Varying the flake size not only changed the electrochemical properties but also changed the wettability of the exfoliated materials as shown in Fig. 8a. It was found that the hydrophobicity of the water increases as the flake sizes grew larger, with the WCA from small to large flakes being roughly 104°, 113°, 114°, 114°, and 124°, respectively. To further explain the interaction between WSe2 flakes and water, Young's equation (eqn (2)) was then applied. By assuming the constant γlv for a given liquid–air behaviour (i.e. similar water–air tension through all samples) and neglecting the γsv, eqn (2) can be rewritten to represent the work of adhesion (Wsl) according to eqn (10):
Wsl = γlv(1 + cosθ) | (10) |
The applicability of WSe2 nanoflakes in supercapacitors is presented in Fig. 9. The smallest WSe2 flakes (quoted as “106 nm flakes”) were chosen as a 2D binder (an additive) in the supercapacitor electrode, instead of using typical conductive additives and polymer binders.42 We have introduced new concepts by using exfoliated TMD materials as pseudocapacitive binders for an alternative option for high performance supercapacitor electrodes (either typical ones or flexible/free-standing electrodes). Overall, we added 10% WSe2 when preparing an activated carbon electrode. The WSe2 flakes provide van der Waals interaction, through which they can bind with the carbon particles. The CV in Fig. 9a shows the success of using WSe2 as a 2D binder. It is evident that the CV of the activated carbon with WSe2 binder shows a more rectangular shape than the activated carbon without the WSe2 binder, indicating higher capacitive properties and improved electrical conductivity.43 After adding the WSe2 binder, the capacitance increased by about 35 percent at 10 mV s−1 (from 55.8 F g−1 to 75.1 F g−1). It was noted that the rate capability of an activated carbon supercapacitor (without adding WSe2) decreased by 70% after increasing the scan rate to 100 mV s−1, while the activated carbon electrode (with WSe2) decreased by only 40% (see Fig. 9b). This improvement is higher than the results achieved in previous reports, reduced graphene oxide as a 2D conductive binder,7 and far better than the results obtained using the MXene film binder.44 For comparison, the supercapacitor performances of activated carbon with PVDF are presented in Fig. S5.† The supercapacitor performance was then investigated using the EIS technique as shown in Fig. 9c. It can be clearly seen that results for both the “with WSe2 binder” and the “without WSe2 binder” provide a resistance solution (Rs) of 0.3 Ω due to the similar electrolytes used. However, the electrode without the WSe2 binder presents a much greater semi-circle as can be seen in Fig. 9c, suggesting that the WSe2 binder could reduce charge transfer resistance (Rct) at the electrode interfaces, which is in accord with the CV result. Note that the Rct of the activated carbon with the WSe2 binder, and the sample without the WSe2 binder is about 73 Ω and 312 Ω respectively. In the lower frequency regions, the Nyquist plot displays a straight line close to the vertical axis, suggesting ideal capacitor properties.38 Moreover, it is clear that after adding the WSe2 binder, the self-discharging behaviour of the supercapacitor improved by about 9% as shown in Fig. 9d, where the potentials after a 1 h test are about 0.64 V (with WSe2) and 0.58 V (without WSe2). As a final point, we successfully used WSe2 nanoflakes as a pseudocapacitive binder, and the WSe2 can bind the activated carbon particles together as shown in Fig. 9e. The supercapacitor with 10% WSe2 binder shows excellent cycling stability up to ∼90% retention while the pure AC supercapacitor displays only 50% retention after 5000 cycles. Moreover, it is clear that an electrode with WSe2 provides a smooth and flexible surface, which blends without cracking. Meanwhile, an electrode without WSe2 displays a rough surface of agglomerate-activated carbon particles. These results show a great potential for using WSe2 nanoflakes as an electrode binder as well as an excellent potential for the preparation of composite materials in the future development of energy storage technologies.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/d0na00592d |
This journal is © The Royal Society of Chemistry 2021 |