In this work, uniform MnCo2O4.5 nanowires (NWs) on stainless steel foil (SSF) were prepared through a facile, cost-efficient, and eco-friendly hydrothermal method at 120 °C with a post-calcination process in air. The microstructure of MnCo2O4.5 samples could be tuned at different hydrothermal temperatures and quasi-cubes (QCs) were obtained in high yield at 150 °C. The MnCo2O4.5 NW powder peeled off from the SSF delivered an outstanding capacity of 248.62 C g−1 at 1 A g−1 with a capacity preservation of 179.43 C g−1 at 8 A g−1, while the QCs exhibited 177.19 and 111.73 C g−1, respectively. To assess the possibility of its actual applications, a hybrid supercapacitor (HSC) device has been assembled by utilizing these MnCo2O4.5 NWs (QCs) and activated carbon (AC) as the cathode and anode, respectively. The MnCo2O4.5 NWs//AC HSC delivered a maximum capacity up to 116.95 C g−1 and extraordinary cycling durability with only 3.56% capacity loss over 5000 cycles. Besides, the MnCo2O4.5 NWs//AC HSC achieved a maximum energy density of 25.41 W h kg−1 at a power density of 782.08 W kg−1, and for the QC-based HSC, it showed a lower energy density of 20.54 W h kg−1 at 843.34 W kg−1. These remarkable electrochemical properties demonstrate that the porous MnCo2O4.5 NWs and QCs may serve as promising cathodes for advanced hybrid supercapacitors with superior performance, and the present synthetic methodology may be applied to the preparation of other cobalt-based binary metal oxides with excellent electrochemical properties.
The energy storage of EDLC electrode materials was achieved through the physical electrostatic charge accumulations in the vicinity of interfaces between the electrode and electrolyte, and no charge transfer during the charging–discharging cycles.10 Carbonaceous materials are among the typical EDLC electrode materials, and they are extensively studied because of their naturally large specific surface area and they exhibit almost no volume change over long-term cycling processes.11,12 However, the relatively low specific capacitance may limit the practical application of EDLC electrode materials in some fields where high energy density is required. In pseudo-capacitive electrode materials, the energy storage mechanism is dominated by rapidly reversible faradaic reactions of electrode materials with electrolyte.13 Metal oxides such as ruthenium dioxide (RuO2) and manganese dioxide (MnO2) are widely known to display typical pseudo-capacitive behavior.14 Moreover, the charge storage of battery-type electrode materials is mainly contributed by the faradaic process which is controlled by ion diffusion kinetics. The main difference is that pseudo-capacitive materials are characterized by EDLC-like electrochemical responses such as distorted rectangle cyclic voltammetry (CV) curves and triangular galvanostatic charge–discharge (GCD) curves, whereas battery-type materials exhibit both a CV curve with obvious redox peaks and a nonlinear GCD curve with an overt plateau region.15
According to the characteristics of electrode materials, supercapacitors are categorized as symmetric supercapacitors (SSCs) and asymmetric supercapacitors (ASCs). The SSCs, such as AC//AC devices, are mainly assembled using the same materials in the cathode and anode through weight matching over charge conservation. However, the low voltage window and rapid attenuation of capacitance along with current density increase limit their widespread applications. In contrast, the ASCs can exhibit wider operating voltage windows and further lead to enhanced capacity/energy density because of the combined contributions from different electrode materials. Particularly, ASCs assembled with battery-type materials as the cathode and carbon-based materials as the anode are called hybrid supercapacitors (HSCs), and the HSCs are expected to show improved energy storage capability.16
The electrochemical performance of electrodes plays a significant role in charge storage capability of HSCs. Thus, the key to improving charge storage behavior of HSCs is the controllable fabrication of hierarchical porous active materials with high specific capacity. To date, cobalt-based binary transition metal oxides (BTMOs) with spinel structures, such as MgCo2O4,17 NiCo2O4,18 ZnCo2O4,19,20 CuCo2O4,15,21 and MnCo2O4.5,22 have drawn considerable interest as supercapacitor electrode materials because of their rich valence states, synergistic effects between mixed metal cations, and enhanced capacity features. Among these BTMOs, MnCo2O4 and MnCo2O4.5 are the most promising battery-grade electrode materials, since the high theoretical specific capacities are mainly ascribed to the multiple valence states of Mn and Co as well as their synergistic influence. But the relatively low conductivity restricts their further wide application to a certain extent. Although significant research efforts have been made with regard to MnCo2O4.5, it is still difficult to achieve its high theoretical specific capacity or extensive operating potential window.23 Up to now, various microstructures of MnCo2O4.5 have been reported. For instance, urchin-like MnCo2O4.5 with diameter ranging from 4–6 μm was synthesized through a hydrothermal approach and it showed only a capacity of 64.6 C g−1 (129.2 F g−1).24 Liao and coworkers prepared spindle-like MnCo2O4.5 microstructures via a solvothermal approach, and the specific capacity of the MnCo2O4.5 microspindles (MSs) was calculated to be 147.49 C g−1 (343 F g−1).25 Cage-like MnCo2O4.5 NPs were prepared through a soft-template assisted method with a calcination process at 600 °C. These irregular MnCo2O4.5 NPs exhibited a poor energy storage capability with 119.2 C g−1 (149 F g−1, 0–0.8 V) at 0.2 A g−1, but lost 41.7% of the initial capacity as the current density was enhanced 20 times.26 Kuang and coworkers reported the growth of MnCo2O4.5 nanoneedle arrays on nickel foam via a hydrothermal route, and a high capacity up to 517.9 C g−1 could be obtained from these MnCo2O4.5 mesoporous nanoneedle structures.27 These efforts not only demonstrate that the efficient way to improve energy storage capability and structural stability is controllable preparation of MnCo2O4.5 mesoporous architectures, but also supply an approach to achieve controlled synthesis of MnCo2O4.5 with an appropriate structure providing more redox active sites. Although growing the active material on a substrate can easily control its morphology, the substrate may influence the final capacity to a certain extent. The specific capacities of some MnCo2O4.5-based electrode materials are listed in Table 1.
Morphology | Specific surface area (m2 g−1) | Pore size (nm) | Specific capacity | Ref. |
---|---|---|---|---|
MnCo2O4.5 microspindles | 83.3 | 8.5 | 147.49 C g−1 at 0.5 A g−1 (343 F g−1, 0–0.43 V) | 25 |
Urchin-like MnCo2O4.5 | 22.4 | — | 59.4 C g−1 at 1 A g−1 (118.8 F g−1, 0–0.5 V) | 24 |
Pod-like MnCo2O4.5 | 73.7 | 12.3 | 138.03 C g−1 at 1 A g−1 (321 F g−1, 0–0.43 V) | 22 |
MnCo2O4.5 nanoneedles | — | 6.2 | 517.9 C g−1 at 3.6 A g−1 | 27 |
Particle-like MnCo2O4.5 | 97.8 | — | 105.6 C g−1 at 1 A g−1 (132 F g−1, 0–0.8 V) | 26 |
Co3O4/MnCo2O4.5 core–shell polyhedra | — | — | 286.2 C g−1 at 1 A g−1 (636 F g−1, 0–0.45 V) | 36 |
MnCo2O4.5@GQDs nanoneedles | — | — | 812.5 C g−1 at 1 A g−1 (1625 F g−1, 0–0.5 V) | 31 |
MnCo2O4.5 NWs@δ-MnO2 nanosheets | 42.3 | — | 357.5 C g−1 at 0.5 A g−1 (357.5 F g−1, −0.2–0.8 V) | 40 |
Grass-like MnCo2O4.5 NWs | 47.03 | 13.27 | 248.62 C g−1 at 1 A g−1 | This work |
MnCo2O4.5 QCs | 62.64 | 7.3 | 177.19 C g−1 at 1 A g−1 | This work |
In this work, we hydrothermally synthesized MnCo2O4.5 with different microstructures on a stainless steel foil (SSF) substrate by changing the hydrothermal reaction temperature. The SSF-supported MnCo2O4.5 has some negative effects when serving as a binder-free electrode material for supercapacitors. It usually possesses large resistance, and the shape exhibits a rigid plate without a three-dimensional porous structure, which may weaken the electron transport and ion diffusion. Particularly, the composition of stainless steel foil from different producers varies, and the accurate composition is difficult to control. In strongly alkaline media, corrosion is probably generated in stainless steel foil more or less, leading to a relatively poor performance of energy storage. Considering the above, the MnCo2O4.5 samples were peeled off from the SSF substrate and the related powder samples were obtained. Grass-like MnCo2O4.5 nanowires (NWs) showed a capacity as high as 248.62 C g−1 at 1 A g−1. Meanwhile, 72.17% of the original capacity was preserved as the current density was boosted from 1 to 8 A g−1, indicating an outstanding rate performance. An HSC device with a high operating voltage of 1.75 V in a strongly alkaline electrolyte was assembled using MnCo2O4.5 NWs as the cathode and AC as the anode, respectively. The MnCo2O4.5 NWs//AC HSC displayed both a high energy density of 25.41 W h kg−1 at a power density of 782.08 W kg−1 and a superior cycling stability with 96.44% capacity retention over 5000 cycles at 4 A g−1.
(1) |
In which I (A) corresponds to the discharging current, Δt (s) denotes the discharging time, and m (g) stands for the mass of MnCo2O4.5.
(2) |
In which m+ and m− mean the weights of active materials loaded on cathode and anode electrodes, respectively. Cs− represents the specific capacitance (F g−1) of the anode electrode, ΔV− corresponds to the potential of the charge–discharge curve, and Qs+ means the capacity of the cathode electrode. The specific capacity of the HSC (CHSC) and its related energy density (E, W h kg−1)/power density (P, W kg−1) are obtained on the basis of eqn (3)–(5), respectively.15,29 The units of specific capacity are C g−1 herein.
(3) |
(4) |
(5) |
In which I (A) is the constant current used in the HSC, Δt (s) corresponds to the discharge time, M (g) means the gross weight of MnCo2O4.5 NWs and AC on the positive and negative electrodes, and t1 and t2 stand for the preliminary time after IR drop and ending time of the discharging process, respectively.
TEM and high-resolution TEM (HRTEM) characterization studies were performed to acquire insights into the morphology and microstructure of MnCo2O4.5 NWs. Fig. 2a shows the TEM image of a MnCo2O4.5 NW with a diameter of approximately 100 nm. Meanwhile, it could be seen that the individual NW was assembled by numerous nanoparticles (NPs). Plenty of pores between the adjacent NPs were also observed, and they could facilitate the diffusion of electrolyte ions. The selected area electron diffraction (SAED) pattern (Fig. 2b) showed that the ED rings consisted of dispersive spots, indicating the polycrystalline characteristic of these MnCo2O4.5 NWs. The high-resolution TEM image shown in Fig. 2c exhibits distinct lattice fringes with different orientations. The close-up high-resolution TEM image (Fig. 2d) for the selected position in Fig. 2c shows an interplanar spacing of 0.234 nm, which is well ascribed to the (222) crystal planes of cubic spinel MnCo2O4.5.
The elemental valence states of MnCo2O4.5 NWs were further identified through X-ray photoelectron spectroscopy (XPS) analysis, and Fig. 3 presents the corresponding XPS spectra. The binding energies of Co 2p, Mn 2p, and O 1s were revised by referring them to the 284.6 eV of C 1s. The full survey XPS spectrum (Fig. 3a) confirmed the coexistence of Co, Mn, and O. As depicted in the Co 2p XPS spectrum (Fig. 3b), the characteristic peaks of Co 2p1/2 and Co 2p3/2 were centered at 795.3 and 780.1 eV (energy gap: 15.2 eV), accompanied by two shake-up satellite peaks at 786.4 and 803.2 eV. It indicated the coexistence of cobalt species including Co2+ and Co3+ in the MnCo2O4.5 NWs.25,30 By refined fitting, the two major peaks in the Co 2p spectrum could be divided into four sub-peaks using the Gaussian fitting method, and the peaks at 781.7 and 797.1 eV were assigned to Co2+, whereas the peaks at 780.0 and 795.2 eV were ascribed to Co3+. Similarly, two closely adjacent peaks at 641.9 and 653.5 eV were observed in the fitted XPS spectrum of Mn 2p (Fig. 3c), which correspond to Mn 2p3/2 and Mn 2p1/2. The fitted peaks at the positions of 641.6 and 653.2 eV were ascribed to Mn2+, while the other two sub-peaks at 643.5 and 655.2 eV were attributed to Mn3+.31 Furthermore, the O 1s spectrum in Fig. 3d exhibits three fitted peaks at 529.9 (O1), 531.2 (O2), and 532.6 eV (O3), which determined the oxygen in the metal–oxygen bond (Mn/Co–O), the oxygen in hydroxyl groups, and the oxygen in water molecules physically and chemically absorbed on the surface of MnCo2O4.5 NWs, respectively.32 On the whole, the XPS data proved that Co2+, Co3+, Mn2+, and Mn3+ appeared simultaneously in MnCo2O4.5, and it also directly confirmed the successful preparation of MnCo2O4.5 NWs in a highly pure phase through an easy and cost-effective hydrothermal route with post-annealing treatment.
Fig. 3 (a) XPS survey spectrum of the MnCo2O4.5 NW powder separated from stainless steel foil and high resolution XPS spectra for (b) Co 2p, (c) Mn 2p, and (d) O1s, respectively. |
There are some parameters including concentration of chlorates, hydrothermal temperature, and the dosage of NH4F and urea which may play significant roles in the growth of MnCo2O4.5 microstructures with diverse shapes. In this work, control experiments were conducted at different hydrothermal temperatures. As shown in Fig. 4, the SEM images displayed the morphological changes of different MnCo2O4.5 microstructures prepared at various hydrothermal temperatures. Fig. 4a shows that the clusters of grass-like MnCo2O4.5 microstructures were homogeneously distributed on the SSF substrate when the hydrothermal temperature was as low as 100 °C, but the yield was not high to some extent. After 6 h of reaction at 100 °C, the solution in the autoclave still remained pink, suggesting that the reaction was not totally completed. A large amount of NWs were obtained at 120 °C (Fig. 1b). When the temperature was increased to 130 °C, a few MnCo2O4.5 quasi-cube (QC) microstructures emerged in the NWs (Fig. 4b). The QCs were composed of a lot of microflakes, and some cusps of NWs on the surface of layered QCs were also observed. MnCo2O4.5 QCs gradually dominated in the products with the increase of hydrothermal temperature (Fig. 4c). Finally, the grass-like MnCo2O4.5 NWs completely disappeared as the temperature was further increased to 150 °C, and these QCs possessed three edges perpendicular to each other (Fig. 4d). As the temperature was increased, the reactions proceeded more rapidly, leading to the formation of less anisotropic QCs. To synthesize micro-/nano-structures with a more anisotropic shape, the reaction should proceed slowly enough in order that the initial nucleation stage can be isolated from the subsequent crystal growth stage. Anisotropic MnCo2O4.5 NWs as the sole final product could be obtained at temperatures below 120 °C.
The porosity and pore size distribution as well as the surface area for MnCo2O4.5 NWs at 120 °C and MnCo2O4.5 QCs at 150 °C were examined utilizing N2 adsorption–desorption isotherms, and the isotherms in Fig. 5a and c were categorized as type-IV with an obvious type-H3 loop, indicating the typical mesoporous nature of MnCo2O4.5 samples. The BET specific surface area of MnCo2O4.5 NWs was evaluated to be 47.03 m2 g−1, and the corresponding pore size distribution was found to be centered at 8.7 nm with an average pore size of 13.27 nm. The existence of mesopores confirmed the observation from the TEM image. In contrast, the MnCo2O4.5 QCs possessed a BET specific surface area of 62.64 m2 g−1, a smaller BJH average pore size of 7.38 nm and a main pore size of approximately 7.3 nm. Obviously, the specific surface areas increased with the shape of MnCo2O4.5 changing from NWs to QCs. Similarly, both the average pore size and main pore size distribution of MnCo2O4.5 QCs were smaller than those of MnCo2O4.5 NWs. The QCs exhibit a very large size of about 10–15 μm (Fig. 4d), and smaller pores may be generated in the inside during the calcination process. In comparison, the NWs are relatively thin in diameter, and they can experience sufficient calcinations, resulting in larger pores as well as smaller surface area.
The electrochemical storage performances of MnCo2O4.5 NWs and QCs were investigated in a three-electrode system through CV, GCD and EIS tests. The typical three-electrode configuration contained the Ni foam loaded with MnCo2O4.5 powder scraped from the SSF substrate, Hg/HgO, and Pt-foil as the working, reference, and counter electrodes, respectively. Freshly prepared 2 M KOH solution served as the electrolyte. As exhibited in Fig. 6a and b, the CV curves of MnCo2O4.5 NWs and MnCo2O4.5 QCs were obtained at different scan rates (5–50 mV s−1) under potential windows between 0 and 0.75 V. All CV curves exhibited a similar shape with a couple of well-defined cathodic and anodic peaks, indicating that MnCo2O4.5 NWs and QCs delivered an obvious battery-type electrochemical response rather than pseudo-capacitive (quasi-rectangular CV curves) or EDLC-type (rectangular CV curves) electrochemical behavior. The plausible redox reactions can be described as follows:31
MnCo2O4.5 + H2O + OH− ↔ MnOOH + CoOOH + e− | (6) |
MnOOH + OH− ↔ MnO2 + H2O + e− | (7) |
Meanwhile, the cathodic/anodic peaks shifted to more negative/positive directions with an increase of scan rate, respectively, which could be mainly ascribed to the polarization at high sweep rate. These observations suggested that fast and reversible faradaic reactions proceeded at the electrode–electrolyte interface, which well matched with that reported in previous literature.33 Furthermore, the CV curves of MnCo2O4.5 NWs exhibited higher cathodic and anodic current densities as well as an apparently larger integrated area compared with those of MnCo2O4.5 QCs, indicating that the MnCo2O4.5 NW electrode possessed higher specific capacity than MnCo2O4.5 QCs. Fig. S1† provides the curves of peak current (ip) vs. the square root of scan rate (v1/2) for both MnCo2O4.5 NWs and QCs, and the proportional relationship indicated that the charge storage procedure was governed by ion diffusion. In addition, the capacitive contribution can be determined using i(V) = k1ν + k2ν1/2. At a fixed potential V, the total current response i can be divided into both the current resulting from capacitive reactions (k1ν) and the current induced by diffusion-controlled reactions (k2ν1/2). After determining the k1 and k2 constants, the quantitative analysis in Fig. S2a and b† indicated that the capacitive contributions were 85% and 88% of the entire charge storage for MnCo2O4.5 NWs and QCs at 40 mV s−1. With the scan rate increasing from 5 to 50 mV s−1, the capacitive contribution for MnCo2O4.5 NWs increased from 56% to 92% (Fig. S2c†), while for the QCs, the value improved from 59% to 93% accordingly (Fig. S2d†).
GCD measurements were carried out to study the specific capacity and rate performance of the MnCo2O4.5 NWs and QCs, and Fig. 6c and d present the corresponding GCD curves at different current densities in the potential window of 0–0.55 V. The specific capacity of MnCo2O4.5 NWs was calculated from eqn (1) and it delivered the values of 248.62, 232.42, 207.12, 192.24, and 179.43 C g−1 at 1, 2, 4, 6, and 8 A g−1, respectively. In comparison, the MnCo2O4.5 QCs exhibited specific capacities of 177.19, 156.35, 132.03, 123.73, and 111.73 C g−1 at each current density, respectively. The specific capacity of MnCo2O4.5 NWs was higher than that of MnCo2O4.5 QCs. The remarkably enhanced specific capacity of MnCo2O4.5 NWs could be ascribed to the existence of mesopores in the thin NWs, which generated numerous channels for ion diffusion and electron transport. However, for the MnCo2O4.5 QC electrode material, due to the huge total size of QCs, the diffusion of ions and electrons was hampered in the inside of QCs, and therefore, slower reaction kinetics could occur during the charge–discharge process. Fig. 6e shows the GCD curves of NWs and QCs at 1 A g−1, and obviously the discharge time of NWs was longer than that of QCs, suggesting the higher capacity of NWs. Fig. 6f illustrates the relationship between specific capacity and corresponding current density. It was clear that capacity decreased with current density increasing, which could be explained by two reasons. On the one hand, a large voltage drop always appears at high current density, and it may cause negative influence on the capacity. On the other hand, inadequate contact between MnCo2O4.5 and the electrolyte was also negative for the contribution of capacity because of the short discharging time at high current density.
To further evaluate the internal resistance and reaction kinetics of the MnCo2O4.5 NWs and QCs, EIS tests were carried out at frequencies between 0.01 Hz and 100 kHz under an open circuit potential by applying an AC voltage of 5 mV amplitude. The Nyquist plots of MnCo2O4.5 NWs and QCs at room temperature are shown in Fig. 7, which were fitted with an equivalent circuit. The equivalent circuit comprised an internal resistance Rs (including the intrinsic resistance of MnCo2O4.5, contact resistance between MnCo2O4.5 and Ni foam, and ionic resistance of KOH aqueous electrolyte), an electron transfer resistance Rct, and a Warburg resistance W. The Rs was directly determined from the intercepts of the X-axis, and the values for MnCo2O4.5 NWs and QCs were found to be 0.81 and 0.67 Ω, respectively. With respect to the Rct resistance, the determined values for NWs and QCs were 0.83 and 0.76 Ω. Both the MnCo2O4.5 NWs and QCs in this work exhibited much lower Rs values than the previously reported Mn/Co-oxide-based materials.26,27,34 In addition, the slope of the straight line at the low frequency region reflected Warburg resistance, which was influenced by the ion diffusion in faradaic reactions between the interface of MnCo2O4.5 electrodes and KOH electrolyte. It indicated the good conductivity of both MnCo2O4.5 NWs and QCs.
Fig. 7 The Nyquist plots of MnCo2O4.5 NWs and QCs, and the inset shows the enlarged plots in the high-frequency region as well as a fitted equivalent circuit. |
In order to investigate the actual application of porous MnCo2O4.5 NWs and QCs, a hybrid supercapacitor (MnCo2O4.5 NWs//AC HSC and MnCo2O4.5 QCs//AC HSC) device was assembled with the NWs (QCs) and AC as the cathode and anode, respectively. As we reported previously, the AC used herein possessed a specific capacitance of 178.5 F g−1 (−1.0–0.0 V) at 1 A g−1 and splendid rate durability (retained 87% of the original capacitance at 16 A g−1),2 illustrating that the AC was suitable as the anode material for supercapacitor applications. The optimal weight ratio of m+/m− was determined according to eqn (2). To achieve the optimal electrochemical properties of the HSC, a series of CV tests were conducted at a scan rate of 10 mV s−1 with the voltage varying between 0–1.2 and 0–1.8 V to ascertain the voltage window of the MnCo2O4.5 NWs//AC HSC. The CV curves obtained with the voltage window of 0–1.8 V (Fig. S3a†) showed a distinct polarization phenomenon. The GCD curves shown in Fig. S3b† were recorded under various voltage windows from 0–1.2 to 0–1.75 V at 1 A g−1, and all GCD profiles displayed a typical feature of quasi isosceles triangle with an imperceptible IR drop. As a consequence, the appropriate operating voltage window of the MnCo2O4.5 NWs//AC HSC was demonstrated to be 0–1.75 V. Fig. S3c† illustrates the specific capacities under different voltage windows, and the capacity increased from 62.34 C g−1 at 0–1.2 V to 116.95 C g−1 at 0–1.75 V. Moreover, energy density showed an upward trend from 10.76 to 25.41 W h kg−1 accordingly (Fig. S3d†).
CV and GCD measurements of the MnCo2O4.5 NWs//AC HSC were carried out within the voltage window of 0–1.75 V. Fig. 8a shows that all the corresponding CV curves manifested a distorted rectangular shape containing broad redox peaks, and the shape remained unchanged with the increase of scan rate, indicating a characteristic capacitive behavior caused by the assembly of battery-type and EDLC electrodes. Symmetrical GCD curves with a nonlinear nature as shown in Fig. 8c were obtained with a variety of current densities, and the plateau region on these curves verified the existence of faradaic reactions during the charge–discharge process. Meanwhile, the specific capacity of the MnCo2O4.5 NWs//AC HSC was calculated through eqn (3), and the values could reach 116.95, 103.80, 92.96, 87.34 and 82.44 C g−1 at 1, 2, 4, 6 and 8 A g−1, respectively. Approximately 70.49% of the initial capacity was retained when the current density was raised from 1 to 8 A g−1, indicating that the MnCo2O4.5 NWs//AC HSC possessed a good rate capability. To make a comparison, the MnCo2O4.5 QCs//AC HSC was also assembled with a fabrication process similar to that of the MnCo2O4.5 NWs//AC HSC, and CV and GCD measurements were performed under the same conditions (Fig. 8b and d). Compared with the MnCo2O4.5 NWs//AC HSC, the MnCo2O4.5 QCs//AC HSC exhibited lower specific capacities of 87.67, 75.93, 65.70, 61.42, and 56.90 C g−1 accordingly. Fig. 8e directly provides the GCD curves of the HSCs at 1 A g−1, which clearly exhibited the longer discharging time of the MnCo2O4.5 NWs//AC HSC than that of the MnCo2O4.5 QCs//AC HSC. The rate performances of both NW- and QC-based HSCs are shown in Fig. 8f, respectively.
It is generally known that the cycling property of HSC devices plays a vital role in determining the actual application of electro-active electrode materials. Repeated GCD tests were performed to study the cycling performance of MnCo2O4.5 NWs//AC and MnCo2O4.5 QCs//AC HSCs at 4 A g−1, as presented in Fig. 9. Over 5000 continuous cycles, the MnCo2O4.5 NWs//AC HSC device exhibits a long-term cycling durability with 96.44% retention of its initial capacity. The inset in Fig. 9a displays the last ten cycles, and no obvious changes in the symmetrical curves were observed, demonstrating an excellent cycling durability of the MnCo2O4.5 NWs//AC HSC. In addition, the MnCo2O4.5 QCs//AC HSC maintained a specific capacity from the initial 65.70 to final 64.25 C g−1 after 5000 cycles, suggesting 97.79% capacity retention. The coulombic efficiency (η) can be calculated using eqn (8), and both the HSCs achieved almost perfect η values (∼100%) during the entire 5000 GCD cycles.
(8) |
Fig. 9 Cycling tests and coulombic efficiency of (a) MnCo2O4.5 NWs//AC and (b) MnCo2O4.5 QCs//AC HSCs during 5000 cycles at 4 A g−1, and the insets provide the last ten GCD curves. |
The Ragone plots of MnCo2O4.5 NWs//AC and MnCo2O4.5 QCs//AC HSCs are illustrated (Fig. 10) along with a comparison of some Mn/Co-based asymmetrical supercapacitors (ASCs) reported in recent literature. The corresponding energy density and power density were obtained through eqn (4) and (5). The MnCo2O4.5 NWs//AC HSC achieved an energy density of 25.41 W h kg−1 at a power density of 782.08 W kg−1 and still retained 18.18 W h kg−1 even at a higher power density of 6.35 kW kg−1. In contrast, the MnCo2O4.5 QCs//AC HSC exhibited a lower energy density of 20.54 W h kg−1 at 843.34 W kg−1. As illustrated in the Ragone plots, the MnCo2O4.5 NWs//AC HSC possessed superior or comparable energy density to the MnCo2O4.5 QCs//AC HSC and some other ASCs assembled with battery-type Mn/Co-based oxides as the cathode, such as MnCo2O4 nanorods//AC (12.77 W h kg−1 at 138.40 W kg−1),35 MnCo2O4.5 pods//AC (19.65 W h kg−1 at 810.64 W kg−1),22 Co3O4/MnCo2O4.5//nanoporous carbon (23 W h kg−1 at 796 W kg−1),36 Ni0.5Mn0.5Co2O4 nanoflowers//AC (20.2 W h kg−1 at 700 W kg−1),37 and NiMnCoO4//reduced graphene oxide (NiMnCoO4//rGO, 20 W h kg−1 at 377 W kg−1).28 However, the value was still inferior to some of the ASCs such as MnCo2O4.5@graphene quantum dots//reduced graphene oxide (MnCo2O4.5@GQDs//rGO, 44 W h kg−1 at 66 W kg−1),31 MnCo2O4 nanosheets//AC (33.8 W h kg−1 at 318.9 W kg−1),38 and MnCo2O4 porous spheres (PSs)//starch-derived carbon foam (SCF) (42.27 W h kg−1 at 400 W kg−1).39 Based on the above electrochemical performances of MnCo2O4 NWs and the corresponding HSC, the porous MnCo2O4 NWs herein can provide a promising application as an advanced battery-grade electrode material for high-performance HSC devices.
Fig. 10 Ragone plots of the MnCo2O4.5 NWs//AC HSC, MnCo2O4.5 QCs//AC HSC, and some other related ASCs reported previously. |
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/d1na00271f |
This journal is © The Royal Society of Chemistry 2021 |