Nhat Xuan An Nguyena,
Le Viet Hai*a,
Thi Kim Ngan Nguyena,
Thi Nam Phamb,
Thi Thom Nguyenb,
Le Thanh Nguyen Huynha,
Van Viet Phama,
Thi Thu Trang Nguyenb,
Nguyen Thai Hoanga and
Tran Dai Lam*bc
aHCM City University of Science, Vietnam National University HCM City, 227 Nguyen Van Cu, HCM City, Vietnam. E-mail: lvhai@hcmus.edu.vn
bInstitute for Tropical Technology, Vietnam Academy of Science and Technology, 18 Hoang Quoc Viet, Hanoi, Vietnam. E-mail: tdlam@itt.vast.vn
cGraduate University of Science and Technology, Vietnam Academy of Science and Technology, 18 Hoang Quoc Viet, Hanoi, Vietnam
First published on 25th August 2021
Graphene sheets decorated with nickel or copper oxides that were anchored on polyaniline (denoted as PANI-graphene/NiO and PANI-graphene/CuO) were prepared by a simple, easy to-control electrochemical method and applied as novel materials for sensitive and selective methanol sensing. The fabricated sensors exhibited good electrocatalytic activity, appropriate dynamic linear range (20–1300 mM), sensitivity (0.2–1.5 μA mM−1 cm−2) and excellent selectivity towards methanol. It should be highlighted from the selectivity tests that no significant interference was observed from ethanol and other alcohols. To our best knowledge, using inexpensive but efficient transition metals like Ni, Cu instead of Pt, Pd and their composites with PANI, graphene would be scientifically novel and practically feasible approach for sensor fabrication that could be potentially used to identify methanol adulteration in counterfeit alcoholic beverages.
Development of a simple/economical, but sensitive/selective as well as practical/label-free method is essentially demanded for environmental monitoring, food industry and clinical diagnostics.3,4 Traditional methods for the quantitative analysis of MeOH including chromatography – mass spectrometry (GC-MS), gas chromatography – flame ionization detector (GC-FID), headspace – gas chromatography (HS-GC), however, these methods required the complex and expensive apparatus, and therefore incompatible for practical routine monitoring of MeOH.5 Over the past decade, MeOH sensors have been proposed as an alternative method for MeOH detection due to their rapid response, low cost, and portability.5–7 These sensors can be classified into two groups based on the mechanism of operation including physical (density, capacitance, viscosity, sound velocity, infrared/Raman spectroscopy, refractive index, heat capacity) and electrochemical types. The low selectivity of the physical sensors linked to similarity in physical properties of alcohols has limited their application. Otherwise, the (electro)chemical sensors offer many advantages thank to their electrical output signal, sensibility, and selectivity. So far, most electrochemical MeOH sensors are developed based on the operating characteristics of the liquid-fed direct MeOH fuel cells (DMFCs). These fuel cell type sensors are very useful for monitoring the concentration of MeOH in the DMFCs. However, this remains extremely difficult for other applications such as the analysis of MeOH in beverages and fuels. While the other approach based on enzyme-modified electrodes (biosensors) remains the challenge of low selectivity as well as stability. Therefore, it is essential to develop simpler and more practical techniques for directly detecting MeOH in the liquid phase.
In this context, the development of non-enzymatic electrochemical sensors using various materials including polymers,8,9 metal10 and metal oxide11–14 nanoparticles (NPs), carbon-based materials and their composites12,15–17 has been intensively explored. In particular, metal and metal oxide NPs, such as Pt,18 Cu,19,20 CuO,11,21 and Pd22 NPs, have attracted significant attention because of their high surface energy and large surface area and thus high electrochemical catalytic activity in numerous electrochemical processes, including methanol electrooxidation. Normally, these NPs are loaded onto the inorganic/organic supports as electrochemical catalysts. It is of crucial importance to ensure both even dispersion and good electron transfer between the surface of NPs and electrode to get higher sensitivity and lower detection limit. Typically, some inorganic–inorganic, organic–organic, inorganic–organic configurations have been proposed such as palladium–nickel/silicon nanowires (Pd–Ni/SiNWs);22 NiO/Fe2O3;23 Au–Ni/graphene oxide;24 graphene–NiO nano composites;25 polymethyl methacrylate–graphene–carbon nanotubes;26 reduced graphene oxide/ferricyanide;27 N-5-methoxysalicylaldehyde, N′-2-hydroxyacetophenone – 1,2 phenylenediimino nickel(II) (Ni(II)–MHP) and reduced graphene oxide (RGO) (Ni(II)–MHP/RGO);28 EG/rGO/np–NiOOH;29 PTh-α-Fe2O330… Although Pt and Pt-based catalysts are common and efficient for MeOH oxidation, there are some significant obstacles preventing their large-scale application such as high cost, reactivity, and the extent of poisoning towards MeOH.
Primary objective of this work is to construct nanocomposite of PANI–graphene to get the appropriate sensitivity, higher selectivity (against other alcohols) for MeOH determination. Despite polyaniline (PANI) is among one of the most widely investigated conductive polymers because of its interesting redox properties, high stability and ease of preparation and graphene is considered as one of the most interesting materials due to its excellent characteristics including its high conductivity. On the other hand, graphene is well-known as a planar sp2 carbon nanostructure that could render the high surface area, outstanding electrical, thermal, and mechanical properties. Moreover, using less expensive but equally efficient transition metals like Ni, Cu instead of Pt, Pd and their composites with PANI, graphene should be also a much more promising approach. For these reasons, PANI–graphene/NiO (or CuO) platforms can be foreseen with following advantageous features: (i) PANI–graphene is capable of eliminating the main drawbacks of the electrochemical sensors such as the phenomenon of “electrode fouling” or “memory effect” from one sample to another as well as the possibility to be produced inexpensively and controllably at large scale; (ii) PANI–graphene interface is expected to express a synergic effect to the overall system and thus improve sensing characteristics; and (iii) the enhanced oxidation of MeOH is likely to occur more favorably at PANI–graphene/NiO (or CuO) compared to that of other alcohol interferences, making the MeOH sensor highly selective and electrochemically feasible. According to the available literature, to the best of our knowledge there is no previous report on the design of PANI–graphene, NiO or CuO catalyzed electrodes for electrochemical detection of liquid methanol from the alcohol mixtures.
The Raman spectra of the samples exhibit two distinct peaks at around 1350 and 1590 cm−1 corresponding to the well-defined D band and G band, respectively (Fig. 2a). The graphitic peak (G band at 1590 cm−1) is due to the E2g vibrational mode of the C–C bond stretching and the disorder peak (D-band at 1350 cm−1) is due to the A1g vibrational mode. The intensity ratio of the D and G bands (ID/IG ∼0.93) allows to estimate the defects of graphene where a lower ratio ensures less defects on graphene. Moreover, from Raman spectra, it can be expected that a strong interaction between PANI and graphene will facilitate effective degree of electron delocalization, and thus enhance electron transfer and the selectivity of electrochemical detection with PANI/graphene interface compared to that of pure PANI. Logically, Raman spectra intensity was weaker for PANI–graphene/CuO (or NiO), after subsequent electrodeposition and electrooxidation. SEM images confirmed high porous structure of PANI–graphene, which is important for Ni (or Cu) occupancy after the electrodeposition (Fig. 2b). Further HRTEM images showed that the Ni or Cu nanoparticles were successfully incorporated onto PANI–graphene nanocomposites (Fig. 2c). The existence of graphene in porous structure can provide a larger specific surface area than pure PANI. The next steps of electrodeposition/oxidation of Ni/NiO (or Cu/CuO) on the surface of PANI–graphene (Fig. 2d and e) were also visualized and compared by FTIR, XRD, EDX analyses of PANI, PANI–graphene and PANI–graphene/NiO (or CuO) composites (Fig. S1–S3, Table S1, ESI†). In summary, on the basis of the above characterization results, it can be concluded that: (i) graphene facilitated electron transport on the electrode surface; (ii) the porous framework of PANI–graphene can be beneficial for Ni or Cu electrodeposition as well the enhanced electron transfer throughout the interface; (iii) enhanced oxidation of MeOH should be expected on synergic PANI–graphene/NiO (or CuO) platform.
Fig. 2 (a) Raman spectra; (b) SEM image; (c) HRTEM image of PANI–graphene/Cu, and (d and e) CV curves for electrodeposition and electrooxidation of Ni, Cu on PANI–graphene. |
CuO/NiO + OH− → CuOOH/NiOOH + e | (1) |
CuOOH/NiOOH + MeOH + 3O2 → CO2 +Cu(II) + 4H2O | (2) |
It is well known that the electrooxidation processes of MeOH and EtOH are very similar to each other and are kinetically slow. From the CV curves, it can be seen that the oxidation potential peak of MeOH (Epeak at 0.8 V) is slightly lower than that of EtOH (Epeak at 0.85 V), but the respective current intensity of the former is much higher than that of the later. Significantly higher peak current densities recorded with MeOH clearly demonstrated the importance of NiO/CuO in MeOH electrooxidation (the electroactivity difference between PANI–graphene and PANI–graphene/CuO in alkaline medium was compared in Fig. S4†). Theoretically, to obtain the highest signal (the largest current), the applied potential in chronoamperometry should be fixed at MeOH oxidation peak potential (0.8 V), however, to deliberately eliminate the involved process of EtOH (to have the best signal/noise), the chronoamperometric curves were recorded at lower onset oxidation potential (0.55 V).
Some important remarks could be drawn from Fig. 4. First, both PANI–graphene/NiO and PANI–graphene/CuO had no response to all added interferences, including EtOH (50 mM added). The electrooxidation of MeOH was significant compared to that of other interferences (EtOH, IPA, acetone): the current intensity for MeOH oxidation (added 50 mM, i ∼3.5 μA cm−2) was greater than that of other interferences at high concentration (200 mM, i < 0.5 μA cm−2). It could be supposed that the detection of MeOH was quite selective even at high concentration of interferences (Fig. S5, ESI†).
Next, since Ni/NiO particles were electrodeposited in a greater quantity on PANI–graphene compared to that of Cu/CuO (see Fig. 2d: the reduction current of the first cycles during metallic electrodeposition), the MeOH oxidation on PANI–graphene/NiO should be more sensitive compared to that on PANI–graphene/CuO for a low MeOH concentration range, as it was experimentally confirmed from the slope values of calibration plots (Fig. 4d, for concentration below 100 ppm). At higher MeOH concentration range, the response currents of PANI–graphene/NiO and PANI–graphene/CuO resembled each other, confirming the same sensitivity for Cu and Ni in that concentration range. The similar electrocatalytic of Ni and Cu in MeOH oxidation can be explained by their similarities in the crystallographic data (both with the same face centered cubic (fcc) structure and lattice parameters) and surface properties. Furthermore, the calibration plots displayed two different slopes related to two linear zones, corresponding to two different ranges of MeOH concentrations: (i) lower concentration from 0 to 400 ppm and (ii) higher concentration from 400 to 1300 ppm, in which the sensitivity decline observed at higher MeOH concentration is likely related to the saturation of the electrocatalytic active sites with MeOH target molecules. The main electroanalytical parameters obtained from different MeOH sensors were compared and summarized in Table 1.
Sensor interfaces | Range (mM) | Sensitivity (μA mM−1 cm−2) | Ref. |
---|---|---|---|
PANI–graphene/NiO | 20–100 | 1.5 | This work |
300–1300 | 0.2 | ||
PANI–graphene/CuO | 20–300 | 0.8 | This work |
300–1300 | 0.2 | ||
EG/rGO/np-NiOOH | 10–40 | 1.32 | 29 |
Graphene/NiO/GCE | 0.2–24 | 2.21 | 25 |
Pd–Ni/SiNWs | 0–75 | 1.96 | 22 |
PMMA–graphene–CNTs | 1 × 10−6 to 10 | 13.494 | 26 |
PTh-α-Fe2O3/GCE | 5–1000 | 0.793 | 30 |
Pt/CNTs | 25–100 | 6 | 11 |
To determine the practical performance and feasibility of the above sensor, the determination of MeOH from real samples of alcoholic beverage was examined. Taking into account the fact that Cu was almost two times cheaper than Ni, PANI–graphene/CuO was chosen for further evaluations with real samples. The results were summarized in Table 2. The recoveries of the samples were in range of 85–99%, indicating that the detection procedure can be used as an effective electrochemical determination of MeOH in the commercial samples.
Parameter | S1 | S2 | S3 |
---|---|---|---|
a Value was obtained by the appropriate dilution factor equal 1/6.b Average of three replicates. | |||
0.1 M NaOH volume (mL) | 30 | 30 | 30 |
Added real sample (mL) | 6 | 6 | 6 |
MeOH conc. (ppm) in real sample | 2500 | 3700 | 4900 |
Diluted MeOH conc.a (ppm) in electrochemical cell test | 416.6 | 616.6 | 816.6 |
MeOH foundb (ppm) (before diluted of real sample) | 2479 | 3187 | 4175 |
Recovery (%) | 99 | 86 | 85 |
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/d1ra04164a |
This journal is © The Royal Society of Chemistry 2021 |