aInstitute of Engineering Thermodynamics/Electrochemical Energy Technology, German Aerospace Center (DLR), Pfaffenwaldring 38-40, 70569 Stuttgart, Germany. E-mail: aldo.gago@dlr.de; Fax: +49 711 6862-747; Tel: +49 711 6862-8090
bInstitute of Engineering Thermodynamics/Computational Electrochemistry, German Aerospace Center (DLR), Pfaffenwaldring 38-40, 70569 Stuttgart, Germany
cDepartment of Mechanical and Industrial Engineering, Faculty of Applied Science and Engineering, University of Toronto Institute for Sustainable Energy, University of Toronto, Toronto, Ontario M5S 3G8, Canada
dFraunhofer-Institut für Solare Energiesysteme ISE, Heidenhofstraße 2, 79110 Freiburg, Germany
eInstitute of Building Energetics, Thermal Engineering and Energy Storage (IGTE), University of Stuttgart, Pfaffenwaldring 31, 70569 Stuttgart, Germany
First published on 7th October 2021
Proton exchange membrane water electrolysis (PEMWE) is the most promising technology for sustainable hydrogen production. However, it has been too expensive to compete with current state-of-the-art technologies due to the high cost of titanium bipolar plates (BPPs) and porous transport layers (PTLs). Here, we report a high-performance, durable and low-cost PEMWE cell with coated stainless steel (ss) BPPs and PTLs. When using uncoated ss components in the PEMWE cell, the cell depolarizes rapidly, reaching 2 V at only 0.15 A cm−2. After the application of non-precious metal coatings of Ti and Nb/Ti on the ss-BPP and ss-PTL, respectively, the current density can be increased by a factor of 13 while maintaining the same performance. Extensive physical and electrochemical characterization supported by pore network modelling shows that the Nb/Ti coating on the ss-PTL leads to efficient water and gas transport at the interface with the anode. The PEMWE cell with coated ss components was evaluated in an accelerated stress test (AST) for more than 1000 h. No sign of Fe contamination in either the membrane or the electrodes is observed at the end of the test. With our results, we demonstrate that PEMWE cells can be manufactured almost entirely in ss, facilitating an unprecedented cost reduction in this technology and advancing the widespread use of green H2.
Broader contextGlobal warming due to high CO2 emissions worldwide is one of the greatest challenges of the 20th century. In the last few years, it has become clear that the current political agreements and efforts will probably not contribute to a sufficient reduction of CO2 emissions. Besides energy and heat generation, the chemical industry and the mobility sector are some of the largest emitters of CO2. Alternatives to the use of fossil fuels must be found for the respective sectors and integrated into the processes in order to stop the steady upward trend. It is therefore essential to tighten up the already ambitious targets set out in the Paris Agreement and to push ahead the expansion of renewable energies. However, energy supply based on renewable energies entails dependence on weather conditions and geographical locations. Both, wind and sun, are not necessarily available when and where energy is needed. Here, hydrogen production via water electrolysis using renewable electricity (green hydrogen) can decouple energy production from actual demand in terms of time, and energy can thus be stored. Proton exchange membrane water electrolysis (PEMWE) is the most suitable technology for this purpose but is still expensive and mainly due to the use of titanium for manufacturing stack components such as bipolar plates (BPP) and porous transport layers (PTLs). Herein, we report a PEMWE cell that is almost fully made of stainless steel, exhibiting high performance and durability. As BPPs and PTLs are made of titanium, the most expensive components of the electrolyzer stack, a significant cost reduction in this technology has been achieved by showing that they can be manufactured in stainless steel. This PEMWE cell with stainless steel components will contribute to the widespread production of green hydrogen. |
The main components of a PEMWE cell are the catalyst coated membrane (CCM), porous transport layers (PTLs) and bipolar plates (BPPs). The CCM consists of iridium and ruthenium oxides (IrOx–RuOy) as the anode and platinum nanoparticles supported on carbon (Pt/C) as the cathode. Besides the BPPs, the PTL is one of the key components of a PEMWE cell that allows effective transport of reactant water to the electrodes while facilitating gas removal towards the flow field of the BPP. Efficient gas/water management has a high impact on the cell performance due to the reduction in mass transport losses.5–7 On the cathode side, carbon paper is a state-of-the-art PTL material, which is often used in PEM fuel cells (FC).8 On the anode side, titanium is widely used for PTLs since titanium can withstand the harsh conditions of a highly concentrated O2 environment and elevated cell potentials (>2 V).3 Commercially available PTLs for the anode include sintered powders, felts, and meshes sold by companies such as GKN Sinter Metals, Bekaert and Melicon, respectively. Recent developments have included tunable PTLs with controlled porosities9,10 and pore structures with a size gradient.11,12
Manufacturing sophisticated porous structures such as sintered powders or felts in titanium is cost prohibitive. Moreover, to avoid passivation, which leads to an increase in cell voltage over time,13,14 titanium must be coated with platinum group metals (PGMs). A stainless steel PTL (ss-PTL) would be preferable, but it severely corrodes, thus poisoning the CCM with Fe and Ni.15,16 Our previous developments have demonstrated that it is possible to use ss as a base material for manufacturing the BPP. A dense coating applied by plasma spraying provides full protection against corrosion in the aggressive PEMWE environment.17 These coatings have been integrated into commercial electrolyser stacks and tested for more than 1000 h without the ss substrate showing any signs of corrosion.18,19 Likewise, physical vapor deposition (PVD) applied Ti/TiN coatings on steel components could be considered for anode-side application in PEMWE cells, which have already been evaluated for their suitability by N. Rojas et al.20 However, a test in a real PEMWE cell was not carried out here. Complementing the anode-side use of the Nb/Ti coated steel BPP, Shirvanvian P. et al. see laser-treated 316L stainless steel, carbon-based and nitride coatings on stainless steel, as already investigated for the PEMFC cell, as possible components for cathode-side use as the BPP in PEMWE cells.21
Depending on the cell configuration, e.g., with or without a flow field in the BPP, the PTL and the BPP together approximately represent between 70%22 and 60%23 of the PEMWE stack cost. The cost of Ir catalyst is the other key cost driver in PEMWE systems and it will become increasingly important as the large-scale manufacturing cost of PTLs and BPPs is reduced. There have been some attempts to use ss-PTLs in PEMWE cells. J. Mo et al. tested an uncoated mesh type ss-PTL in a PEMWE cell.16 The ss-PTL corroded rapidly and the realised Fe poisoned heavily the CCM. Another attempt was made by N. F. Daudt et al. in which they sintered a Nb coating on a ss-PTL.24 From their PEMWE tests, one can notice that the slopes of their polarization curves with the coated ss-PTL bend sharply upwards at ca. 1 A cm−2, which is an indication of either mass transport losses or severe degradation. The authors do not report any stability test though.
A complete PEMWE stack manufactured mainly in ss, that is, PTLs and BPPs, remains an important challenge. Such a stack could drastically reduce the PEMWE cost for large-scale applications, making green hydrogen more competitive. In this work, we report the first efficient, stable and high performance PTL made of ss coated with non-precious Nb/Ti metal by plasma spraying. The coating not only protects the PTL against corrosion but also significantly improves the cell performance. Through extensive characterization and numeric simulation, we provide a comprehensive explanation of this improved performance. The coated ss-PTLs in combination with our previous development of coated ss-BPPs allow the production of a PEMWE cell with all metallic components made of ss, thus marking an unprecedented cost reduction in this technology.
Fig. 1 Scheme of the ss-mesh PTL with a plasma-sprayed Nb/Ti coating at the interface with the anode catalyst layer. |
(1) |
X-ray CT analysis was performed with a multi-scale X-ray nanotomograph (Skyscan 2211, Bruker). The reconstructed sample volume was 484.4 × 1386 × 1649.9 μm3, achieving a resolution of 0.7 μm. An acceleration potential of 70 kV was used.
(2) |
In contrast, such as the setup in Fig. 2b, the anode and cathode water loops of the BoP are kept as simple as possible. There are no ss pipes, pumps or any other metal parts in which ions could redeposit. The inlets and outlets of the cell are connected to small volume water reservoirs that are opened to the air. The water is fed to the cell via natural flow and the water level is kept constant by filling periodically with fresh water. This setup does not contain an ion exchange resin. Therefore, in this setup, any Fe2+ released due to the corrosion of Nb/Ti/ss-PTLs will rapidly poison the CCM as the water volume is kept small and constant. Any other impurities in the DI water, such as Ca2+, Cu2+, Na1+, organics and metal ions in the ppm range, also continuously increase with each refill. Consequently, the cells with either Ti-PTL or coated ss-PTL will rapidly degrade, but the degradation rates will be different if the ss PTL substrate corrodes. Therefore, this setup can be well used for an AST in which water purity is the main stressor.
The AST setup was employed for evaluating the Nb/Ti/ss-PTL in PEMWEs with an active area of 4 cm2. On the anode side, the following interconnecting components were used: a ss-BPP with a dense coating of Ti,19 and a Nb/Ti/ss-PTL, and for the cathode side: an uncoated multi-layer mesh-type ss-PTL (Haver & Boecker OHG) and a ss-BPP. All stainless steel components were of 1.4404 grade. An untreated carbon paper (TGP-H-90) was placed between the cathode electrode and the ss-PTL. CCMs with an Ir-based anode, Pt-based cathode and chemically stabilized Nafion 115 membrane were used for all electrochemical tests, except for the test of Fig. 10. The loading of the catalyst is 2.5 mg cm−2 for iridium and 0.95 mg cm−2 for platinum. Polarization curves up to 2 A cm−2 with a scan rate of 4 mA cm−2 s−1 and electrochemical impedance spectroscopy (EIS) spectra were obtained at 0.25 and 1 A cm−2 and an amplitude of 50 mA and 200 mA, respectively, from 50 kHz to 100 mHz. A potentiostat/galvanostat (Zahner Elektrik IM6) with a booster (Module PP240) was used for these measurements, which were carried out at 65 °C and ambient pressure. The Nb/Ti/Ti-PTL, uncoated Ti-PTL and ss-PTL were also measured for comparison purposes. Once the polarization curves and the EIS were completed, a constant current of 2 A cm−2 was applied for an AST for more than 1000 h.
Fig. 3 Scanning electron microscopy (SEM) images of Ti-PTL (a) without and (b) with plasma-sprayed Nb/Ti coatings and ss-PTL (d) without and (e) with plasma-sprayed Nb/Ti coatings. Cutaway images of Nb/Ti on (c) Ti-PTL and (f) ss-PTL, which correspond to the blue dashed squares in (b) and (e). The solid-line squares in (c) and (f) indicate the areas where EDS was carried out, and the results are summarized in Table 1. |
Area designation | O [wt%] | Si [wt%] | Ti [wt%] | Cr [wt%] | Fe [wt%] | Ni [wt%] | Nb [wt%] | Mo [wt%] |
---|---|---|---|---|---|---|---|---|
MW 1 | 2.36 | — | 0.91 | — | — | — | 96.73 | — |
MW 2 | 2.37 | — | 0.79 | — | — | — | 96.85 | — |
MW 3, 4, 5, 6 | — | — | 100.00 | — | — | — | — | — |
MW 7 | 3.10 | — | 0.35 | — | — | — | 96.55 | — |
MW 8 | 3.32 | — | 0.57 | — | — | — | 96.12 | — |
MW 9, 10 | — | — | 100.00 | — | — | — | — | — |
MW 11 | 0.71 | 0.39 | 0.54 | 16.99 | 68.93 | 10.03 | — | 2.40 |
MW 12 | 0.69 | 0.31 | 0.21 | 17.50 | 69.57 | 9.44 | — | 2.28 |
First, the Ti layer covers almost the entire surface of the fine-mesh ss substrates, which is particularly important for protecting the PTL against the corrosive environment in the vicinity of the anode catalyst layer. Subsequent layers of Ti are porous to allow the transport of reactants and products from the water splitting process. The Ti particles of the porous layer do not form the conventional splat structure that one can observe in the dense Ti coatings17 due to their low enthalpy during the plasma coating deposition. However, the Ti particles have a certain degree of inter-particle diffusion among each other, ensuring the mechanical stability of the coating. On top of the Ti porous layer, Nb uniformly follows the rugosity of the coating composed of Ti particles. Nb functions as an anti-passivation coating for Ti,19 which is an alternative to costly precious metals that are normally used for extending the lifetime of PEMWE cells. It is worthwhile noting that the Nb/Ti coating slightly reduces the gaps of the punched holes in the ss fine mesh, which can improve the catalyst utilization of the electrode.9,31
One important aspect regarding the corrosion resistance of the Nb/Ti coatings is the purity of Ti and Nb. EDS was carried out on different cross-sectional areas of the coated PTLs. These areas are indicated as red rectangles and labelled MW in Fig. 3c and f for Nb/Ti/Ti-PTL and Nb/Ti/ss-PTL, respectively. The results of the EDS analysis are summarized in Table 1. The SEM image of Fig. 3c shows almost no colour contrast between the Ti particles (MW 3) and the Ti-mesh substrate (MW 5), suggesting that they both have the same elemental composition. The EDS results confirm that Ti-mesh substrates are pure Ti and can be considered Ti Gd1, which is the standard material for the PTL in PEMWE. Conversely, the MW 10 and 11 areas in Fig. 3f show deep contrast since these areas correspond to two very different materials, ss and Ti. The brightest material in the image corresponds to Nb. The anti-passivation layer of Nb also has a high degree of purity, and the presence of less than 1 wt% Ti is most likely attributed to the fluorescence of Ti since the measured area is quite close to the Nb/Ti interface. While EDS is not a suitable technique for measuring elements with low atomic mass, the presence of oxygen can be disregarded because during the plasma deposition process oxygen combines with the feedstock H2 gas to form H2O.
In addition to the optimized pore properties of Nb/Ti/ss-PTL, a good electrical connection between the plasma-sprayed coating and the catalyst layers ensures high performance due to low ICR. The ICR measurements of the Nb/Ti/ss-PTL, Nb/Ti/Ti-PTL, and uncoated PTL substrates with respect to the compaction force are presented in Fig. 5. The method for estimating the ICRs of the plasma-sprayed coatings has been previously reported,11,19 and the experimental setup is schematized in the inset of Fig. 5. A thin sheet of carbon paper is placed between the PTLs and one of the Au-coated Cu cylinders. The ICR between the Nb/Ti coating and the anode catalyst layer can be approximated by using a carbon paper sheet instead of the Ir-based layer, as both have high in-plane electrical conductivity. Furthermore, carbon paper acts as a material that can be compressed in the applied range of compaction forces.
Fig. 5 Interfacial contact resistance (ICR) with respect to the compaction force of Ti-PTL, ss-PTL, Nb/Ti/Ti-PTL and Nb/Ti/ss-PTL. The inset shows a scheme of the experimental setup. |
First, Fig. 5 reveals that all PTLs have relatively the same ICR, which is approximately 100 mΩ cm2 at a compaction force of 150 N cm−2, corresponding to the compression of the PEMWE cell during the assembly. This result is quite remarkable, although it might be characteristic of only multi-layer mesh-type PTLs. In contrast, Bernt et al.32 and Kang et al.33 report different resistance values between different PTLs, with and without MPL coating. For this kind of PTL, the Nb/Ti coatings have essentially no influence at all in the ICR of the PTL, and this effect should be reflected in the PEMWE tests. However, we will demonstrate in the next section that the Nb/Ti coating has a strong influence on the performance of the PEMWE in which the coating reduces ohmic losses at high current densities.
Fig. 6a shows the ECell–j characteristics of a PEMWE cell with the ss-PTL, Nb/Ti/ss-PTL, and Nb/Ti/Ti-PTL and the ECell values at a constant 2 A cm−2. We observe that the use of an uncoated ss-PTL causes rapid cell depolarization, reaching up to 2.28 V at only 0.4 A cm−2. The cell is only operated up to this current density, and therefore, the ECell at a constant 2 A cm−2 is not plotted. The PEMWE cell becomes inoperable afterwards, turning the feedstock water into a yellowish solution, similar to the colour of the electrolyte used for evaluating ss-BPPs under simulated conditions of a PEMWE cell. These results provide clear evidence for the magnitude of the challenge when using ss as a base material for the manufacture of a low-cost PTL.
In stark contrast, by coating the ss-PTL with Nb/Ti in PEMWE cells, it is possible to achieve performances comparable to those of commercial electrolysers, such as those from Hydrogenics,34 Siemens35 and Proton Onsite.36 Clearly, the Nb/Ti coating not only protects the ss-PTL against corrosion but also has a staggering influence on the cell performance. To understand this effect, a PEMWE cell with a mesh-type Ti-PTL similar to the ss-mesh was also tested. The mesh-type Ti-PTL is the lowest cost PTL in the market, but it leads to low performances, as shown in Fig. 6a and b. Consequently, most PEMWEs use Ti felts and sinter powder plates as PTLs, although these are much more expensive than a Ti punched mesh due to the manufacturing process. First, an interesting observation is that there are large differences in the slope of the polarization curve of Ti-PTL and those of Nb/Ti/ss-PTL and Nb/Ti/Ti-PTL. At first glance, this result contradicts the observations from the ICR measurements, which show no difference in ohmic resistance among all the PTLs. Second, the polarization curve of the cell with the Ti-PTL shows a hysteric behaviour, while for the others, the forward curve overlaps with the one measured backwards. Finally, the Nb/Ti coating reduces the ECell by more than 300 mV at 2 A cm−2 compared with that of the uncoated Ti-PTL. This decrease in the overpotential represents an efficiency increase of approximately 12%, which has an important impact on the cost of hydrogen production. EIS will provide comprehensive explanations for all these phenomena. It is important to remark that the mesh Ti-PTL cannot be considered a baseline as the cell performance is too low compared to other well-known baselines such as the Ti felt and sintered Ti plates. However, the Ti mesh is considerably cheaper than the felt or the sintered structures and even more so is a stainless steel mesh. As a consequence, there is lot of interest from the industry to use this kind of PTL and it has potential to become the new PTL baseline in PEMWE cells. In this work we aim to use the lowest cost materials available, that is stainless steel meshes and plates to construct the PEMWE cells, and the achieved performances are comparable to other reports that use baseline sintered Ti-PTLs.31,37 In Fig. S2 (ESI†) we show a comparison between the polarization curve of Nb/Ti/ss-PTLs in Fig. 6a and the one from a baseline Ti-PTL from GKN Sinter Metals,38 which is commercial, and having a Pt coating applied via magnetron sputtering PVD.19 The resulting curves show that the performances of the PEMWE cells with the Nb/Ti/ss-PTL and the baseline Pt/Ti-PTL (GKN Sinter Metals) are quite comparable.
The Nyquist plots of the PEMWE cell with the Ti-PTL, Nb/Ti/Ti-PTL and Nb/Ti/ss-PTL at 0.25 and 1 A cm−2 are shown in Fig. 6c and d, respectively. The spectra were analysed based on the equivalent circuit introduced in previous work and are shown in Fig. S3 (ESI†).12 The ohmic resistance is given by the interception of the first semi-circle in the high-frequency region with the x-axis. The resistances induced by the hydrogen evolution reaction (HER),39 charge transfer resistance coupled with double layer effects34 or the first charge transfer of the two-electron process of the oxygen evolution reaction (OER)40 are represented by the high-frequency arc. The medium- and low-frequency arcs thereby describe the charge transfer of the OER rate-determining step and the mass transport losses.41
At 0.25 A cm−2, all three cells show comparable ohmic resistance of approximately 188 ± 1 mΩ cm2, which is in good agreement with the ICR results of Fig. 5. However, the discrepancy between the ICR and EIS could be due to the additional resistance in the catalyst layer depending on its components, such as ionomer and binder, and therefore ICR measurements cannot be directly linked to the measurements from EIS. In general, the curves for the Nb/Ti/Ti-PTL and Nb/Ti/ss-PTL are comparable to each other in their behaviour, while Ti-PTL presents a slightly larger high-frequency arc. For all samples, the second semi-circle that is associated with the OER kinetics is equivalent in size, and only for Ti-PTL there is an appearance of a small third arc with an apex at 0.1 Hz, indicating mass transport losses. In contrast, at 1 A cm−2, the differences in the EIS between the cells with the coated and uncoated PTLs are very noticeable. The first most noticeable change at 1 A cm−2 is the increase in the ohmic resistance for Ti-PTL, while for the Nb/Ti/Ti-PTL and Nb/Ti/ss-PTL, the ohmic resistance remains almost the same at both 0.25 and 1 A cm−2. Another important change in the EIS is the increase in the radius of the medium-frequency semi-circle for Ti-PTL compared to Nb/Ti/Ti-PTL and Nb/Ti/ss-PTL. Finally, the low-frequency arc of Ti-PTL increases drastically, indicating higher mass transport losses, which is in good agreement with the hysteresis shape of the polarization curve in Fig. 6a. Conversely, the mass transport effects for the coated PTLs are barely visible.12
The Nb/Ti coatings have a significant influence on the ohmic resistance, anode performance and mass transport behaviour during PEMWE. The ohmic resistance refers to the transitions of all cell components (PTLs, BPPs, membranes, and catalyst layers); these components should have the lowest possible resistance due to their high contact with each other. On the one hand, this contact can be worsened by the formation of non-conductive passivation layers on the Ti-PTL;42,43 however, on the other hand, insufficient compression and thus insufficient utilization of the possible contact area can also worsen the ohmic resistance. The optimum compression of the components can be reduced by either different material expansion coefficients depending on the temperature or the conceivable formation of a gas cushion between the catalyst layer and PTL. Due to inefficient gas–water management, which can be observed in simple PTLs,44 the produced gas accumulates at the boundary layer and reduces the contact. While no mass transport loss is observed for the coated PTLs, the Ti-PTL is the only sample that shows ohmic loss shifts to higher values; thus, mass transport limitations seem to have a decisive effect on the Ti-PTL.
Nevertheless, it should be noted that the increase in performance due to the application of the Nb/Ti coating is not only caused by the reduction in mass transport losses. The highly developed surfaces of the coated PTLs with their small porous particle layers provide a high interfacial contact area, resulting in low membrane deformation. In contrast, the region of the catalyst layer not in contact with the uncoated PTL surfaces intrudes into the large pore space, becomes degraded and thus loses conductivity. The surface of the anode at the interface between the catalyst layer and Nb/Ti/Ti-PTL or Nb/Ti/ss-PTL is highly active, whereas large areas of the interface between the catalyst layer and Ti-PTL are electrochemically inactive. This is consistent with the EIS results in Fig. 6d, which show improved kinetics of both the HER and OER, for Nb/Ti/Ti-PTL and Nb/Ti/ss-PTL. Furthermore, this finding agrees very well with the results of Schuler et al.,31 who revealed that the advantage of the MPL lies in the local microscopic compression of the catalyst layer, which preserves the electrical catalyst percolation network. In addition to an increase in the catalyst utilization, this can also be understood as a reduction in membrane deformation, resulting in a significant increase in performance. Lopata et al.45 came to the same conclusion and confirmed the dominance of the interface between the PTL and catalyst layer with regard to the cell performance influencing the high-frequency resistance, catalyst utilization, coverage of PTL grains due to gas bubble formation and ionomer conductivity.
PNM was employed to understand the improved mass transport phenomena in PEMWE cells with the addition of the Nb/Ti coatings. The mass transport characteristics of the coated PTLs are described by the simulated drainage curve and the capillary entry pressure of the pores. The drainage curve shown in Fig. 7 exhibits a wide range of entry capillary pressures, from approximately 780 Pa to 100 kPa. During the process of drainage, the non-wetting phase first preferentially invades pores with lower entry (threshold) capillary pressures (i.e., first invades larger pores in the fine mesh substrate). Although a wide range of capillary pressures is required to fully drain the wetting phase, the wetting phase saturation dramatically decreases at the lower end of the capillary pressure curve (shown as a plateau from 1 to 0.1 in Fig. 7).
Fig. 7 Drainage characteristics generated from the pore network simulation results on the coated PTLs, (a) invaded pores and throats at capillary pressures of 3.6 kPa and (b) 99.8 kPa. |
The wetting phase saturation decreases to below 10% at a capillary pressure of 3.6 kPa, indicating that most of the pore space in the coated PTL is composed of pores from the fine mesh substrate. At this capillary pressure, the larger pores (mostly from the fine mesh) are invaded by the non-wetting phase (left inset of Fig. 7), while the smaller pores (at the Nb/Ti coatings) remain uninvaded. The smaller pores become invaded after all the larger pores have been penetrated, as shown in the right inset of Fig. 7, where the small pores from the Nb/Ti coating are invaded with gas at a capillary pressure of 25 kPa. At approximately 100 kPa, the full domain of the coated PTLs becomes saturated with the non-wetting phase. To fully invade the PTL, the gas generated from the OER requires a capillary pressure build-up over an order of magnitude higher than the value to attain a 10% wetting phase saturation, which is unlikely to occur during electrolysis. Instead, the gas will break through to the larger pores in the coarser mesh by establishing a preferential transport pathway, thus leaving small pores in the Nb/Ti coatings uninvaded. Similar observations are reported in the previous literature.46,47 First, Lee et al. revealed via modelling and in operando neutron imaging experiments that having a porosity gradient from low to high porosity facilitates mass transport during electrolysis. Moreover, they further47 demonstrated that when a custom pore structure was applied to the PTL (i.e., pores with diameters excessively larger than the average pores in the PTL), the gas saturation at the catalyst layer-PTL interface was significantly reduced and mass transport behaviour was enhanced particularly at higher current density operation. Therefore, the Nb/Ti coatings in our PTL lead to improved mass transport behaviour – the smaller pore structure (from the Nb/Ti coating) provides additional reactant transport pathways while the larger pore structure (pores from the mesh) provides effective gas removal pathways.
In contrast, during imbibition of liquid water into the PTL, the liquid water will preferentially invade pores with a higher capillary pressure (i.e., smaller pores in the Nb/Ti coating). Therefore, additional transport pathways for reactant water are supplied by the small pores of the Nb/Ti coating. It is anticipated that even at high current densities, gas removal is facilitated through the large pores, and water is transported through the smaller pores in the Nb/Ti coating. In the absence of the small pores inherent in the Nb/Ti coating, reactant transport would be impeded by the gas removal process and lead to mass transport losses.
All three PEMWE cells degrade rapidly, but the cells with the Ti-PTL in particular reach ECell values close to 2.5 V, which we define as the end of test (EoT), in less than 100 h. Basically, two irreversible degradations that lead to an increase in ECell are identified in the literature: (i) an increase in ohmic resistance due to the formation of oxides at the interface of Ti-PTL13,49 at the anode and (ii) CCM poisoning due to impurities in the water.28,50 A third irreversible degradation mechanism is also known, which is the loss of polymeric material in the CCM, but in this case, the ECell decreases over time.34,51 For the short time of the AST, the passivation of titanium is clearly not the dominant degradation mechanism, see Fig. S4 (ESI†), but the CCM poisoning caused by the impurities in the water that increase over time. The test with the cell with the Ti-PTL was stopped at approximately 720 h as the ECell was no longer below the EoT. A different behaviour is observed with the PEMWE cells containing the Nb/Ti/ss-PTL and Nb/Ti/Ti-PTL. The ECell values for both electrolysers have almost identical trends over time, which is a preliminary indication that the ss substrate of the Nb/Ti/ss-PTL is not corroding. Otherwise, the cell with Nb/Ti/ss-PTL should degrade faster than the cell with Nb/Ti/Ti-PTL. The ASTs for PEMWE cells with the Nb/Ti/Ti-PTL and Nb/Ti/ss-PTL were stopped at approximately 1450 h.
At the EoT, a re-assembly procedure was implemented to quantitatively determine how much the ageing of the Nb/Ti/ss-PTL contributed to the overall cell degradation and is shown in Fig. S5 (ESI†). By cleaning all metal cell components and replacing the CCM, the initial cell voltage at constant 2 A cm−2 was almost completely recovered with 99%. Based on these findings, which were also observed by Sun et al.,28 we conclude that the CCM is mainly responsible for the degradation of the cell. Fig. S6 (ESI†) shows the ECellvs. time of a PEMWE cell with Nb/Ti/ss-PTL in a conventional test station with ss pipes, pumps, gas separators, sensors, valves and other BoP components. As expected, the test in this setup does not show any increase in the ECell values due to degradation mechanisms (i) and (ii); rather, the ECell values decrease slightly over time, as is the case of an electrolyser with very stable BPPs and PTLs,34 thus corresponding to degradation mechanism (iii).
An AST alone is still not sufficient to prove that Nb/Ti protects the ss-PTL against corrosion. If there is indeed any release of Fe2+ ions from the ss-PTL, it should be present in the post-tested CCM. Elemental mapping with EDS was carried out on the CCMs of PEMWE cells with Nb/Ti/ss-PTL and Nb/Ti/Ti-PTL that were subjected to the AST in Fig. 8. The results are presented in Fig. 9. The first column of images corresponds to the uncoated ss-PTL just after the first polarization curve shown in Fig. 6a. Fe (coloured in blue) is substantially present in the Ir-based anode, Pt-based cathode and Nafion membrane. In this latter component, the formed Fe crystals are most likely Fe3O415 (see Fig. S7a, ESI†). In stark contrast, the Nb/Ti/ss-PTL (second column in Fig. 9) does not show any apparent traces of Fe in the anode, cathode or membrane, which is the same as the case of the cell with Nb/Ti/Ti-PTL (third column of images in Fig. 9). This characterization of the post-tested CCMs in the PEMWE cells with the coated ss-PTL and ss-BPP for the anode and the uncoated ss-PTL and ss-BPP for the cathode clearly demonstrates that ss can be used as a base material for manufacturing the metal components of the entire electrolyser. Additionally, the SEM images of the uncoated ss-PTL and Nb/Ti/ss-PTL after the AST are shown in Fig. S8 (ESI†). The surface of the ss-PTL was clearly eroded due to the corrosion in the PEMWE cell while for the Nb/Ti/ss-PTL, no sign of degradation can be observed in either the Nb/Ti coating or the ss-PTL substrate. Lastly, X-ray photoelectron emission spectrometry (XPS) measurements, Fig. S9 (ESI†), did not reveal any Fe on the cathode of the CCM of the cell with the Nb/Ti/Ti-PTL that pass from the anode to the cathode across the PEM and inductive coupled plasma mass spectrometry (ICP-MS) of a water sample taken at the end of the test shown in Fig. 8 did not detect any increase of Fe.
Fig. 9 EDX mapping of the (a–c) cross-section of the CCM, (d–f) cathode and (g–i) anode surfaces of the PEMWE cell with the uncoated ss-PTL, Nb/Ti/Ti-PTL, and Nb/Ti/ss-PTL. |
Regarding the cost/scalability of the vacuum plasma spraying technique for the deposition of Nb/Ti on the ss-PTL we have previously estimated a cost for the coating (without Nb) of about 20–100 USD m−2.17 The cost of coating production is significantly low, but it could be decrease further if the coatings are applied in a line of production, where the torch is sweeping and spraying the materials continuously on the substrate, which is either a mesh-type PTL or a flat BPP. The substrates can be produced in large area metal rolls that can be un-folded during the coating process. Industrial plasma spraying processes are scalable but one challenge may be the use of vacuum that contributes to cost that is more sensitive for the electrolysis application than for traditional uses of VPS (e.g. coating of turbine blades or implants). In this regard, further investigations in the future are needed to produce Nb/Ti coatings via atmospheric plasma spraying (APS), without affecting the structure, mechanical integrity and purity of the coatings.
(i) A reduction in the ohmic resistance, which is caused by gas formation at the interface with the anode.
(ii) An improved utilization of the anode catalyst resulting in enhanced OER kinetics.
(iii) A reduction in mass transport losses.
To further understand the observed phenomena, PNM showed that the advantage of the Nb/Ti coating was explicitly due to the preferred transport of water and gas to and from the active surfaces of the anode. With the results presented herein, it can be concluded that Ti can be ruled out as a base material for the manufacture of expensive porous structures for PTLs; instead, low-cost ss meshes can be used. Moreover, ss meshes with different aperture sizes allow the use of flat plates as BPPs, which can also be manufactured in ss, without a flow field. Thus, the cost of a PEMWE cell has been reduced drastically by being almost entirely made of ss, establishing this technology as the most promising solution for the production of green hydrogen from renewable sources.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/d1ee02112e |
This journal is © The Royal Society of Chemistry 2022 |