aGreen Chemistry Network Centre, Department of Chemistry, University of Delhi, Delhi 110007, India. E-mail: rksharmagreenchem@hotmail.com
bDepartment of Chemistry, Hindu College, University of Delhi, Delhi 110007, India. E-mail: dr.anjusrivastava@gmail.com
cDepartment of Chemistry, Hansraj College, University of Delhi, Delhi 110007, India
dChemistry Division, Department of Sciences and Humanities, Vignan's Foundation for Science, Technology and Research (VFSTR), Vadlamudi, Guntur 522 213, Andhra Pradesh, India
eDepartment of Industrial and Engineering Chemistry, Institute of Chemical Technology, Mumbai-Marathwada Campus, Jalna, Maharashtra, India
First published on 6th January 2022
Magnetic covalent organic frameworks (MagCOFs) represent a new class of emerging material, primarily employed in separation applications. Due to their attractive properties such as easy and cost-effective synthesis, high porosity, large surface area, strong π–π interactions between COF shells and facile magnetic recovery, MagCOFs are being widely deployed in adsorption applications and exhibited high adsorption performance. This review emphasizes on the key advancements in the synthesis of MagCOFs and documents their potential in diverse separation applications including nitro explosive treatment, heavy metal ion adsorption and extraction of persistent organic pollutants, poly aromatic hydrocarbons and endocrine-disrupting chemicals, among others. In addition to offering up-to-date research outcomes in the field of separation science by utilizing MagCOFs, this article also highlights the challenges and possible solutions in this exciting developing area of research.
COFs represent a promising class of well-defined porous and crystalline polymeric materials synthesized via condensation reactions of 2D and 3D organic building precursors.9,10 In general, they are composed of light elements such as hydrogen, boron, oxygen, carbon, nitrogen and silicon which are linked via strong covalent bonds in a reversible manner to generate reticular architecture. This thermodynamically controlled and reversible dynamic covalent chemistry of COFs allows “proof reading” and “error checking” during the synthesis and results into the self-healing ability of COFs leading to the formation of long range ordered crystalline structures.11 Additionally, the presence of π–π interactions and hydrogen bonding among COF shells strengthens their porous skeleton and provides long-term stability.3 Recently, COFs have attracted researchers’ interest because of their intriguing properties such as tuneable composition and high thermal and chemical stability (Fig. 1)12,13 and have been widely used in a variety of applications including energy conversion14,15 and storage,16,17 gas storage,18,19 catalysis,20–25 optoelectronics,26,27 sensing,28,29 drug delivery30–32 and adsorption33–35 to name a few.
Despite being recognized as a very promising class of materials at an early stage of discovery of COFs, unfortunately, the progress in the field is restricted due to some challenges. For example, their extraction from the matrix is not very efficient because of their low density which causes difficulty in their separation from reaction medium.36 In addition, their large-scale applications are hampered due to tedious centrifugation and filtration methods. Over the past few decades, several techniques have been introduced to circumvent those challenges such as liquid–liquid phase extraction, Solid-phase extraction, solid-phase micro extraction, Soxhlet extraction and many others.37 However, most of these techniques are often associated with numerous shortcomings, including large amount of toxic solvent consumption, low selectivity, cumbersome filtration and time-consuming procedures.38 Therefore, there is always a need to develop simple, environmentally benign and highly sensitive synthetic techniques which not only provide COFs with greater selectivity but also speed up the recovery process. Recently, magnetic solid-phase extraction (MSPE), a promising modification of SPE, has been developed as the most prominent technique in the field of separation and sample pre-treatment as it offers an easy recovery of adsorbent using a simple external magnetic field, with high extraction efficiency and large adsorption capacity.39,40 Owing to the appealing properties of magnetic nanoparticles (e.g. Fe3O4; MNPs) including cost-effectiveness, reusability, easy operation, facile synthesis, low toxicity and good magnetic performance, they have been further explored in a variety of disciplines and are commonly used as magnetic extraction materials.41–55 Moreover, a wide variety of functional moieties can be grafted over the surface of magnetic nanocomposites, which make further modifications and reactions more convenient. The introduction of magnetism in COFs has proven to be an effective strategy to solve the recovery problem of COFs. Considering the broad diversity, unique capability and wide applications of both magnetic nanoparticles and COFs, we believe that this combination will open up newer avenues in the rational design of core–shell structures with magnetic platforms and tuneable porous COF shells for wide applications.
Henceforth, after witnessing the effectiveness of MSPE, one of the notable approaches to circumvent the issue of separation would be to simultaneously integrate COFs with a magnetic component which would provide the ease of separation. This would give rise to MagCOFs that would combine the merits of rapid separation with adequate binding sites and high adsorption performance with enhanced functionality.38,56–66 More recently, MagCOFs have marked a breakthrough in the current area of COF-related research. In particular, solid spherical magnetic core can offer a center for uniform COF growth and crystallization in all directions, which provides a possibility for controllable synthesis of magnetic core–shell COFs.67 Therefore, synthesis of MagCOFs and the investigation of their in-depth utility in adsorption science has become an area of prime significance in material science.
Reusability and recyclability are the prime features of magnetic composites that controls the economy and efficiency of process at industrial scale. Although the benefits of using COFs as adsorbents are enormous, but their large-scale utility is still hampered due to their expensiveness, cumbersome filtration and centrifugation process used for the recovery of the composite. In this regard, MNPs supported COFs have been utilized as significant adsorbents for environmental remediation. This introduction of magnetism in COFs circumvent the issue of separation and provide the ease of separation.
To check the recyclability of MagCOF composite, numerous adsorption–desorption cycles are performed. In view of this, Cai et al. synthesized magnetic adsorbent (Fe3O4@COFs) and shows excellent stability and reusability even after ten adsorption–desorption cycles.71 Similarly, Li and co-workers utilized Fe3O4@COF@Zr4+ for the extraction and determination of organophosphorus pesticides in vegetables.72 Subsequently, various adsorption–desorption cycles were performed using the same magnetic composite. It is noteworthy that, prior to next cycle the as-synthesized MagCOF was washed with acetone and distilled water. Thus, Fe3O4@COF@Zr4+ can be reused for six cycles without any significant loss in its activity. Hence, the above examples state that MagCOF composite showed admirable reusability, mechanical stability and cost-effectiveness and also advantageous from environmental viewpoints. Table 1 lists the recyclability runs of numerous MagCOFs composites.
S. No. | MagCOF | Saturation magnetization (Ms) | Recyclability runs | Ref. |
---|---|---|---|---|
n.d. = no data. | ||||
1 | Fe3O4@COF | 62.5 | 3 | 148 |
2 | Fe3O4@TpBd | 22 | 5 | 67 |
3 | Fe3O4@COF | 42.7 | 12 | 70 |
4 | Magnetic TpPa-1 | 40.1 | n.d. | 71 |
5 | Fe3O4@COF | 48.4 | 10 | 100 |
6 | M-COF-2 | 15.8 | 5 | 149 |
7 | Fe3O4@COF | 42 | 20 | 114 |
8 | Fe3O4@COF@Au-β-CD | 21.86 | n.d. | 150 |
9 | MagCOF@MIP@CD | 10.97 | 8 | 151 |
10 | COF-(TpBd)/Fe3O4 | 51.8 | 4 | 142 |
11 | SPIO@COF-guanidyl | 42 | 5 | 121 |
12 | Fe3O4@iCOFs | 21.8 | 7 | 122 |
13 | Fe3O4@SiO2@TpPa-Ti4+ | 35.67 | n.d. | 123 |
14 | mTpBd-Me2 | 60.5 | 5 | 152 |
15 | M-DAPS-COF-SH | 19.6 | 5 | 131 |
16 | Fe3O4@COF(TpPa-1) | 19.5 | 5 | 153 |
17 | Fe3O4@COF(TpBD)@Au-MPS | 40.7 | n.d. | 154 |
18 | Fe3O4@TbBd | 41.4 | 10 | 155 |
In view of the attempts to extract EDCs, Zhao et al. recently designed core–shell structured MagCOFs microspheres (Fe3O4@COF) by the reaction of 1,3,5-tris(4-aminophenyl) benzene (TAPB) and terephthaldicarboxaldehyde (TPA) with Fe3O4 as shown in Fig. 2.80 The fabricated Fe3O4@COF microspheres were deployed in the selective extraction of four endocrine-disrupting phenols (4-n-nonylphenol, 4-n-octylphenol, BPA and BPAF) from plastic-packaged food, drinks and environmental water systems using a combination of MSPE with HPLC. The presence of surface functional groups (–COOH, –CN, –NH2) in Fe3O4@COF forms π–π interactions and hydrogen bonds with the specific sites of target molecules, which make them conducive for MSPE to extract target molecule from various samples. The proposed extraction mechanism involves the formation of hydrogen bonds between amino groups as well as CN groups present on the surface of Fe3O4@COF microspheres and the hydroxyl groups of endocrine-disrupting phenols. Moreover, due to the presence of amino groups on Fe3O4@COF, the polarity and hydrophilicity of the particles gets improved, resulting in additional enhancement in extraction proficiency. Additionally, because of the large logKow (it is a ratio value without a unit and defines solubility of substance in water) and pKa values of endocrine-disrupting phenols, they have a great tendency to escape from the water phase to the surface of Fe3O4@COF. Finally, the efficacy further increases due to the presence of π interactions between aromatic rings of COF shells and aromatic rings of endocrine-disrupting phenols. Besides, the indicative mesoporous structure of Fe3O4@COF also plays a vital role in the adsorption process by providing large surface area with appropriate surface functionalities. The excellent extraction performance is also attributed to the hydrophobicity of the material and the ionization of endocrine-disrupting phenols. Also, the other factors that ascribed to high adsorption performance of MagCOFs are hydrogen bonding, superparamagnetism, electrostatic interactions and ion-exchange. Besides, the coordination reaction between composite materials and pollutants is also a key parameter. The method earned excellent linearity (R ≥ 0.995) within the concentration range of 0.05–1000 ng mL−1. The limit of detection (LOD) and limit of quantification (LOQ) were in the range of 0.08 ng mL−1 to 0.21 ng mL−1 (S/N = 3) and 0.39 ng mL−1 to 0.85 ng mL−1 (S/N = 10), respectively. Besides, the magnetic adsorbent showed high saturation magnetization (62.5 emu g−1) and can be used for 20 runs without any loss in its adsorption capacity. The experimental data revealed that MagCOFs possess great potential as MSPE adsorbent for extracting various other pollutants from food. Hence, after the adsorption of pollutants using MagCOFs, the external magnet was used to assist their separation from aqueous media i.e., if external magnet was removed, the MagCOF composites were dispersed again within a few seconds.
Fig. 2 Synthesis of Fe3O4@COF and extraction of EDCs. Reproduced with permission from ref. 80. Copyright 2019 Springer Nature Publishing AG. |
Likewise, Li and co-workers designed sensitive and efficient core–shell MagCOFs (NiFe2O4@COFs) via facile room temperature ultrasonic approach and the resulting magnetic nanocomposites were utilized for effervescent reaction-enhanced microextraction of endocrine disruptors in liquid matrices (Fig. 3).81 The equilibrium adsorption capacity of six EDCs on magnetic adsorbent were found to be between 38.3 and 88.1 mg g−1 which were primarily attributed to π–π interaction between analytes and MagCOFs. Moreover, NiFe2O4@COFs showed Ms value of 17.1 emu g−1. The magnetic nanocomposites effervescent reaction-enhanced microextraction (MNER-EM-HPLC-FLD) method had good linearity in the range of 0.1–0.5–200 μg L−1, high precision (relative standard deviations (RSDs) of 3.11–5.73%), good recoveries (83.4–106.2%) with lower LOD (0.019–0.096 μg L−1) and R2 (0.8952). Additionally, NiFe2O4@COFs could be reused for at least six cycles.
Fig. 3 Schematic diagram of the MNER-EM/HPLC-FLD method. (a) Synthesis of NiFe2O4@COF MNCs, (b) preparation of the magnetic effervescent tablets and (c) pre-concentration measurements and analytical procedures of EDCs by the MNER-EM/HPLC-FLD method. Reproduced with permission from ref. 81. Copyright 2020 Elsevier B.V. |
BPA is an another EDC which has been widely used to produce epoxy resins and polycarbonate plastics.82,83 It is a pervasive contaminant which can interfere with endocrine systems of humans, wildlife and environmental health. In addition, it has been reported to induce a decrease in daily sperm count and fertility.84 Thus, the removal of BPA and BPAF through selective and efficient adsorption has gained tremendous attention in recent years. Though numerous adsorption methods have been developed so far, nearly all of them are associated with some drawbacks such as complicated synthetic procedure of the materials, prolonged time period, lower adsorption capacity of the material, slower adsorption kinetics, and many more. In this respect, considering the rising interest in the development of MagCOFs, Yan et al. designed monomer mediated in situ growth strategy for the controllable synthesis of core–shell structured MagCOF nanospheres, Fe3O4@TpBd, for the efficient adsorption and removal of EDCs, BPAF and BPA from aqueous solution (Fig. 4a).67
Fig. 4 (a)Monomer-mediated in situ strategy for synthesis of core–shell structured Fe3O4@TpBd nanospheres, TEM images of (b) Fe3O4, (c) Fe3O4@TpBD and (d) HAADF-STEM image and EDX elemental mapping of Fe3O4@TpBD. Reproduced with permission from ref. 67. Copyright 2017 Royal Society of Chemistry. |
The Fe3O4@TpBd was designed in a very systematic manner: Fe3O4 NPs were initially synthesized via a solvothermal method, afterwards –NH2 groups were introduced on the surface of magnetic core to produce amino functionalized nanospheres (Fe3O4–NH2) to avoid aggregation of MNPs as well as to incorporate polar surface functionalities. Furthermore, a monomer of TpBd, 1,3,5-triformylphloroglucinol (Tp), was grafted over Fe3O4–NH2via Schiff base condensation reaction for in situ growth of COF shell. To acquire uniform crystalline growth of COF shell, pre-grafting of monomer played a crucial role. The pre-grafting of monomer Tp acts as a bridge between magnetic core and COF shell to achieve better interaction and helps to nucleate the centers for uniform COF growth. Further, another monomer benzidine (Bd) was grafted over uniform core–shell through imine bond formation. Additionally, TEM, HAADF-STEM and EDX elemental mapping data confirmed a typical core–shell structure of Fe3O4@TpBd nanospheres (with TpBd thickness being 15–65 nm) (Fig. 4b–d). Moreover, the choice of solvent and concentration of monomers acts as key factors to control the thickness and crystallinity of COF shells.
The as-synthesized Fe3O4@TpBd was then explored for adsorption of BPA and BPAF and displayed higher adsorption capacity with faster adsorption kinetics followed by facile magnetic separation. The adsorption equilibrium was achieved within 5 min for BPA and BPAF. The adsorption isotherms of BPA and BPAF on Fe3O4@TpBD illustrate a typical Langmuir adsorption with the maximum adsorption capacities of 160.6 and 236.7 mg g−1, respectively. Fe3O4@TpBd showed excellent reusability up to five runs, which rendered them as novel adsorbent for aqueous solution adsorption.
In a similar fashion, extraction of BPs from human serum sample using MNPs immobilized COF, Fe3O4@COF, was studied by Lin and co-workers (Fig. 5).70 The core–shell structured magnetic adsorbent was fabricated by immobilizing two building units, TAPB and TPA on the surface of MNPs (of size 250 nm) via Schiff base condensation reaction at room temperature. Further, the adsorption efficiency of Fe3O4@COF (with COF thickness being 25 nm) was investigated by evaluating their adsorption isotherms and adsorption kinetics. Further, to determine the magnetic properties of bare Fe3O4 and Fe3O4@COF, VSM was used. From Fig. 5c, it can be noted that Ms value decreases from Fe3O4 (54.5 emu g−1) to Fe3O4@COF (42.7 emu g−1) which can be attributed to grafting of COF shell over Fe3O4. The inset of Fig. 5c display that Fe3O4@COF nanocomposite was dispersed in aqueous solution and separated with the aid of external magnet within 2 minutes. Besides, thermogravimetric analysis (TGA) of Fe3O4 and Fe3O4@COF showed weight loss of 6% and 48% respectively, which implies high yield of COF shells over MNPs in the temperature range of 100–350 °C. Fe3O4@COF showed excellent thermal stability under 300 °C (Fig. 5d). Moreover, due to high porosity, high thermal and chemical stability and large specific surface area (181.36 m2 g−1) of magnetic adsorbent, equilibrium was attained very quickly, indicating fast adsorption kinetics and size selectivity. The high adsorption of BPs was achieved due to van der Waals forces and strong π–π interactions between COF shells and benzene rings of BPs.
Fig. 5 (a) Preparation of the Fe3O4@COF nanocomposites and (b) MSPE process for extraction of BPs in human serum sample, (c) VSM curves of Fe3O4 and Fe3O4@COFs and (d) TGA curve of Fe3O4 and Fe3O4@COFs. Reproduced with permission from ref. 70. Copyright 2018 Elsevier B.V. |
The developed protocol possessed good linearity in the range of 0.1–50 μg L−1 with R2 ≥ 0.9982. Besides, LODs were found to be between 1.0 to 78.1 ng L−1 with high enrichment factor (56–95-fold). The RSDs were less than 3.4% for inter-day and 6.9% for intra-day. Moreover, the authors assessed the performance of Fe3O4@COF in real samples and satisfactory results were obtained with recoveries ranging from 93.0–107.8%. The additional advantage of the developed adsorbent was its ability to be recycled and reused for twelve adsorption–desorption cycles.
On a similar note, an aptamer functionalized magnetic core–shell structured conjugated organic framework (Fe3O4@COFs-Apt) has been developed for the selective extraction of trace –OH PCBs from human serum sample (Fig. 6a and b).36 An aptamer is a single strand DNA/RNA molecule, having high binding affinity towards target molecule through van der Waals, electron–acceptor–donor and hydrogen-bonding interactions. For the synthesis of Fe3O4@COFs-Apt, firstly, MNPs were synthesized by two conventional methods, i.e., co-precipitation and solvothermal method. To improve chemical stability and to avoid agglomeration, bare MNPs were coated with silica using tetraethyl orthosilicate (TEOS). Relatively inexpensive and simple silica coating not only minimizes the aggregation but also provides many potential benefits such as chemical inertness, high binding strength with iron-oxide core, robustness, possibility for further functionalization, etc.88–95 Further, amino groups were introduced on the surface of Fe3O4@SiO2 to obtain amino-modified Fe3O4@SiO2@NH2. Afterwards, the monomers, p-phenylenediamine (PPD) and trimesoyl chloride (TMC) were added to obtain carboxylic acid rich MagCOFs (Fe3O4@COFs-COOH). Thus, to enhance the extraction efficiency, aptamers were immobilized on the surface of MagCOFs (Fe3O4@COFs-Apt) via covalent linkage between surface carboxylic groups and the amino groups of the aptamers. Fe3O4 with average size of 150 nm were obtained by solvothermal method, denoted as Fe3O4@COFs-Apt-150 and Fe3O4 with an average size of 15 nm were obtained by co-precipitation method and denoted as Fe3O4@COFs-Apt-15.
Fig. 6 (a) Synthetic illustration for the synthesis of Fe3O4@COFs-Apt, (b) typical process for selective extraction of OH-PCBs with Fe3O4@COFs-Apt and (c) comparison of extraction efficiency of 2-OH-CB 124, 4′-OH-CB 112, 4′-OH-CB 61 and 4′-OH-CB 30 with Fe3O4-15, Fe3O4@COFs-COOH-15 and Fe3O4@COFs-Apt-15. Reproduced with permission from ref. 36. Copyright 2018 John Wiley & Sons. |
The N2 adsorption–desorption isotherms revealed that Fe3O4@COFs-Apt-15 had higher surface area and hence considered as a better adsorbent material. Subsequently, Fe3O4@COFs-Apt-15 was deployed for the extraction of hydroxy-2′,3′,4′,5,5′-pentachlorobiphenyl (2-OH-CB 124). To check the selectivity of Fe3O4@COFs-Apt-15 for 2-OH-CB 124, three other compounds such as 4′-hydroxy-2,3,3′,5,6-pentachlorobiphenyl (4′-OH-CB 112), 4-hydroxy-2,3,4,5-tetrachlorobiphenyl (4′-OH-CB 61) and 4′-hydroxy-2,4,6-trichlorobiphenyl (4′-OH-CB 30) were selected to conduct unspecific tests. The results unveiled that Fe3O4@COFs-Apt-15 displayed highest recovery of >90% for 2-OH-CB 124, indicating the superior extraction efficiency of 2-OH-CB 124 (Fig. 6c). The adsorption ability for above four compounds was also investigated with Fe3O4-15 and Fe3O4@COFs-COOH-15 only to obtain satisfactory recoveries with Fe3O4@COFs-Apt-15. The presence of π–π stacking interaction, high surface area and hydrophilic property (raised from carboxylic group) increased the adsorption capacity of Fe3O4@COFs-Apt-COOH-15. Meanwhile, Fig. 6c depicts that in comparison with Fe3O4@COFs-Apt-15, Fe3O4@COFs-COOH-15 could not provide satisfactory selectivity for 2-OH-CB 124 (recoveries <25%), which indicates that aptamer played a substantial role towards selectivity of 2-OH-CB 124 due to their highly specific binding affinity. Under optimized conditions, Fe3O4@COFs-Apt-15 showed great potential in determination of 2-OH-CB 124 from human serum samples with recoveries in the range of 87.7–101.5%. The MSPE-LC/MS coupled method exhibited good linearity in the range of 0.01–40 ng mL−1 with excellent R2 value of 0.9973. The LOD was low (2.1 pg mL−1) with a satisfactory LOQ (6.7 pg mL−1). Besides providing easy magnetic recoverability, the adsorbent could be recycled for ten extraction cycles.
Poly aromatic hydrocarbons (PAHs) are a type of POPs that have long been considered as hazardous for both human and environment. They mainly originate from anthropogenic activities such as pyrolysis of organic materials such as oil, coal, wood and petroleum gas. Due to highly mutagenic, carcinogenic and teratogenic potential of PAHs, they are one of the greatest environmental and economic threats to our society.96 In this regard, Cai et al. fabricated a gypsophila bouquet-shaped MagCOF, TpPa-1, by grafting COF over the surface-modified MNPs, for enhanced extraction of PAHs from environmental samples (Fig. 7).71 The novel TpPa-1 was synthesized by facile room temperature solution-phase approach and utilized the advantageous properties of both MNPs and COF. Initially, surface-modified Fe3O4 nanoparticles (of size 30 nm) were synthesized by pre-grafting of monomer Tp onto amino functionalized Fe3O4 nanoparticles. This process helped in acquiring uniform COF shell by generating COF centers via Schiff base reaction. Further, another monomer, phenylenediamine (Pa-1) was added under mechanical agitation to obtain magnetic TpPa-1. The TEM image in Fig. 7 clearly depicts the gypsophila bouquet-shaped structures of TpPa-1. Magnetic TpPa-1 possessed superparamagnetism (40.1 emu g−1) as well as large surface area and high porosity.
Fig. 7 Synthesis and application of the bouquet-like magnetic TpPa-1 sorbent. Reproduced with permission from ref. 71. Copyright 2017 American Chemical Society. |
The as-synthesized magnetic TpPa-1 was further explored for the extraction of PAHs. Initially, magnetic TpPa-1 was directly dispersed into filtered water sample spiked with PAHs and further subjected to ultrasonication followed by additional shaking for 20 min. After extraction of analytes, the sorbent was gathered using external magnet and the supernatant was subjected to HPLC-FLD system for further detection. Moreover, it was anticipated that TpPa-1 might extract organic targets containing benzene ring, amino or hydroxyl groups due to the presence of high percentage of oxygen and nitrogen atoms as well as large π–π framework. The fabricated nanocomposite exhibited an excellent linear range of 2.0–200.0 ng L−1 with a good R2 of 0.9993, with LOD ranging from 0.24–1.01 ng L−1. Furthermore, the material possessed good reusability and could be applied in real sample analysis including lake water, tap water and river water with percentage recoveries of PAHs over 73–110% with a lower RSD value (2–8%). Inspired by encouraging extraction efficiencies of magnetic TpPa-1 towards PAHs, it is expected that the bouquet shaped MagCOF could also have strong affinity towards other chemicals. Besides, magnetic TpPa-1 can also be utilized in wider applications by post-synthetic modification approach.
Similarly, a new and promising class of COF has been synthesized by Chen and group for PAHs extraction.97 They synthesized COF-LZU1@PEI@Fe3O4via covalent immobilization of COF-LZU1 (imine-based COF, prepared by Schiff base reaction of 1,3,5 triformyl benzene (Tb) and 1,4 diaminobenzene) on PEI-functionalized MNPs (Fig. 8a). Firstly, MNPs were coated with polyethyleneimine (PEI) by electrostatic interactions (PEI@Fe3O4). Thereafter, several active amino groups present on PEI enhanced the covalent bonding between the PEI layer and COF-LZU1, due to which COF shells were grown on the surface of MNPs through Schiff base reaction. The designed method was further applied for the extraction of six PAHs from environmental and real samples by MSPE coupled with HPLC. The concentration level of PAHs in an environmental sample is quite low to determine directly by analytical instrument. So, their pretreatment using MSPE was necessary prior to HPLC. COF-LZU1@PEI@Fe3O4 exhibited high surface area, excellent thermal stability and high porosity, which increased the loading capacity of the adsorbent. As discussed earlier, the presence of aromatic rings and imine groups in COF led to strong π–π stacking and hydrophobic interaction with analytes. These characteristics made them an attractive material for solid phase extraction of PAHs. The TEM images showed that PEI@Fe3O4 and COF-LZU1@PEI@Fe3O4 display beautiful cubic morphology with mean diameter of 40 nm (Fig. 8b and c). Also, it can be noted that surface of PEI@Fe3O4 was smooth and after modification with COF-LZU1, a rough and thin polymer layer was observed (due to porous structure of COF-LZU1) which confirms immobilization of COF-LZU1 over PEI@Fe3O4.
Fig. 8 (a) Synthesis of COF-LZU1@PEI@Fe3O4 and TEM images of (b) PEI@Fe3O4 and (c) COF-LZU1@PEI@Fe3O4. Reproduced with permission from ref. 97. Copyright 2021 Springer Nature Publishing AG. |
To optimize the extraction efficiency, various parameters were investigated, such as the effect of temperature, type of solvent, pH of the sample solution, extraction time and sampling volume. Due to the presence of highly hydrophobic aromatic rings in PAHs, the addition of small amount of acetonitrile facilitates their solubility in aqueous sample solution. Further, it was observed that when acetonitrile content increased from 0.5% to 1%, PAH extraction efficiency increases while it decreases when acetonitrile content increases from 2% to 10%. Hence, results stated that a certain amount of acetonitrile do facilitates the solubility in sample solution. Best extraction was achieved when 1% acetonitrile was used as a solvent. Further, sample pH was investigated from 4.0 to 9.0. It can be noted that as pH varies from 4.0 to 9.0, extraction efficiency of PAH increases. This is because H+ can affect the interaction between PAH and adsorbent. Then, with decrease in pH value, the –NH2 groups present on COF-LZU1 would change to NH3+ and this would decrease the π-electron cloud density and weak π–π stacking interaction by its electron-withdrawing inductive effect. Thus, for better extraction efficiency 9.0 was selected as sample pH value. The extraction time was 30 min with a sample volume of 20 mL. Under optimized conditions, the extraction performance of COF-LZU1@PEI@Fe3O4 was evaluated. The results showed that COF-LZU1@PEI@Fe3O4 displayed significant extraction efficiency. The combination of MSPE and HPLC methods showed good linear range with R2 higher than 0.9989. The LOQ was 0.5–50 pg mL−1. Besides, the adsorbent could be reused for up to six cycles. The above research expands the scope of MagCOFs as adsorbents for extraction of various other pollutants.
In this context, Hu et al. fabricated magnetic porous organic polymers (MOPs) via simple azo reaction under mild reaction conditions between monomer, TAPB and 1,3,5-trihydroxybenzene using Fe3O4@SiO2 as the magnetic core (Fig. 9a).37 The as-synthesized MOPs (having 5 nm thick polymer layer) have been utilized as an adsorbent for the extraction of five target TFs (triazolone, penconazole, hexaconazole, diniconazole and tebuconazole) from vegetables by MSPE. For the desorption of TFs, organic solvents with different polarity such as ethyl acetate, acetonitrile, mixed solvents (acetone:ethyl acetate (1:1/v/v)) and acetone were used but best results were obtained when ethyl acetate was used as a desorption solvent. The MSPE-GC-FID showed good linearity in the range of (0.5–200 μg L−1 with R2 > 0.9991–0.9998). The LOD for five target TFs was found to be in the range of 0.12–0.19 μg L−1 according to the three-fold signal-to-noise ratio. Moreover, lower RSDs value (2.6–6.8%), efficient extraction efficiency (84.5–90.3%) and reusability up to five runs demonstrated its excellent performance. The developed MSPE-GC-FID was facile, rapid, selective and sensitive and proved its incredible potential towards extraction of TFs.
Fig. 9 (a) Preparation of MOPs, and (b) Synthesis of Fe3O4@COFs. Reproduced with permission from ref. 100. Copyright 2019 American Chemical Society. |
On this note, Cai et al. fabricated Fe3O4 (MNPs) supported core–shell structured MagCOF, Fe3O4@COF, for the efficient extraction and rapid removal of TCC and TCS from water and serum samples (Fig. 9b).100 To fabricate Fe3O4@COF, MNPs (of size 165 nm) were first synthesized via solvothermal method. Further, COF shell was introduced on the surface of bare Fe3O4 by Schiff base condensation reaction of monomer TAPB and TPA in DMSO at room temperature. Additionally, the adsorption performance of Fe3O4@COF was investigated by Langmuir and Freundlich adsorption isotherms. The Langmuir model was more appropriate in the high concentration region while Freundlich isotherm was more appropriate in the low concentration region. Also, Langmuir and Freundlich isotherms displayed monolayer adsorption at high concentration range and multilayer adsorption at low concentration, respectively. The monolayer adsorption took place due to strong π–π stacking interactions between the interface of TCS, TCC and Fe3O4@COF while multilayer adsorption was due to van der Waals forces, π–π interactions among phenyl rings and space embedding interaction. Moreover, the adsorption kinetics followed a pseudo-second-order kinetic model.
The quantitative analysis of TCC and TCS was determined using UHPLC-MS/MS. The results stated good linearity in the range of 0.05–25 ng mL−1 for TCC and 0.1–50 ng mL−1 for TCS with R2 greater than 0.9976. The LODs for TCC and TCS were 0.005 and 0.02 ng mL−1, respectively. The method was further applied to remove TCC and TCS from healthy fetal bovine serum samples and showed excellent recoveries in the range of 92.9–109.5% and 82.3–95.4% for TCC and TCS, respectively. Moreover, the adsorbent was reused for ten adsorption–desorption cycles with similar extraction efficiency. With the combination of marvellous characteristics of COF and magnificent properties of Fe3O4, Fe3O4@COF served as a potential candidate for the treatment of environmental and biological samples.
Continuing the utility of MagCOFs, Shuai et al. developed a MagCOF via salt-mediated crystallization strategy under solvent free environment for the removal of diclofenac sodium from water. The fabrication procedure involved the grafting of Tp and p-phenylenediamine (PDA) on amino-functionalized MNPs using p-toluenesulfonic acid as catalyst (Fig. 10).107Fig. 10b and c shows narrow size distribution and uniform spherical morphology of Fe3O4 nanospheres with mean diameter of 10–15 nm. Also, the magnetite nanoparticles are tightly shelled by SiO2. Besides, MagCOF-2 shows that MNP-NH2 is well encapsulated in COF framework. Adsorption isotherms displayed a Freundlich isotherm which was well fitted in case of adsorption of diclofenac sodium on MagCOF-2 with a high R2 value (∼0.99) of the curve and a maximum adsorption capacity of 565 mg g−1. The adsorption equilibria were achieved within 20 min indicating the supremacy of MagCOF-2 towards diclofenac sodium removal. The value of Freundlich constant (n > 1) revealed that the adsorption of diclofenac sodium was favourable. Moreover, the experimental data reflected that the effective adsorption is caused by π–π stacking, hydrogen bonding and electrostatic interactions. Additionally, with excellent magnetization and high specific surface area, the as-synthesized magnetic adsorbent could be reused for five cycles without any significant loss of its adsorption capacity. The applicability of MagCOF-2 was also assessed in actual water samples. Interestingly, the results ascribed superior potential of MagCOF-2 for diclofenac sodium removal.
Fig. 10 (a) Synthesis of MagCOF-2 via a solvent free, salt-mediated crystallization strategy, TEM images of (b) MNP-NH2 and (c) MagCOF-2. Reproduced with permission from ref. 107. Copyright 2019 American Chemical Society. |
Similar to the previously discussed MNPs grafted COF, Wang et al. designed few other MagCOFs by facile impregnation method for the removal of diclofenac and sulfamethazine (SMT). For the synthesis, firstly, TPB-DMTP-COFs were synthesized using the reaction between dimethoxyterephthaldehyde (DMTP) and TAPB monomers. Secondly, the as-synthesized TPB-DMTP-COF was reacted with a solution containing Fe2+ and Fe3+ followed by membrane separation. Finally, separated solids were immersed in ammonia solution to yield Fe3O4 in COF structure, (Fig. 11).108 The adsorption activity of the MagCOF was evaluated by adsorption kinetics and isotherms. Adsorption kinetics revealed that equilibria were achieved within 50 min for the removal of diclofenac and 80 min for SMT removal with a maximum adsorption capacity of 40.4 mg g−1 and 55.24 mg g−1, respectively. From the experimental data it was noted that pseudo-first-order model was better in diclofenac adsorption while SMT adsorption was well described by pseudo-second-order kinetic model with R2 > 0.99 in both cases. In addition, the adsorption process of diclofenac and SMT was well defined by Sips isotherm model. By Sips model, the maximum adsorption capacity of diclofenac and SMT was found to be 109 mg g−1 and 113.2 mg g−1, respectively. Furthermore, the adsorption mechanism was studied by density functional theory (DFT) which revealed that the adsorption took place by C–H⋯π interaction. The adsorption energies were calculated to be −47.8 kJ mol−1 and −63.2 kJ mol−1 for SMT and diclofenac, respectively. When the efficacy of the magnetic adsorbent was compared with previously reported adsorbents, MagCOF showed higher adsorption capacity.
Fig. 12 (a) Synthesis of Mag-COF-1 and extraction of paclitaxel, TEM images of (b) M-PEI and (c) Mag-COF-1 and (d) chromatograms of rat plasma samples (A) with extraction and (B) without extraction. Reproduced with permission from ref. 41. Copyright 2016 Elsevier B.V. |
In view of this, Zhang et al. developed porphyrin-based MagCOF (Fe3O4@COF) for the extraction and analysis of six SAs (sulfamerazine (SMR), sulfadiazine (SDZ), sulfamethazine (SMZ), sulfamethoxazole (STZ), sulfamonomethoxine (SMX) and sulfadimethoxine (SDM)).114 For the synthesis, firstly, amino-functionalized MNPs were formed via facile one-pot strategy. Further, COF shells were grown on the surface of amino-functionalized nanospheres using dehydration reaction between two organic ligands namely 4,4′-biphenyldicarboxaldehyde and TAP (Fig. 13a). The presence of amino groups on the surface of Fe3O4 nanospheres facilitated the in situ COF growth via Schiff base reaction. Moreover, the presence of nitrogen containing heterocyclic ring in porphyrin-based COF offers specific multiple-interactions i.e., π–π interaction, hydrogen bonding, hydrophobic and electrostatic interactions with target analytes. Fig. 13b and c showed that the as-obtained Fe3O4@COF (10 ± 2 nm thickness) nanospheres were spherical in shape with average size of 100 ± 14 nm.
Fig. 13 (a) Synthesis of Fe3O4@COFnanospheres, TEM images of (b) Fe3O4, (c) Fe3O4@COF, and chromatograms of six SAs standard solutions (d) before extraction, (e) after extraction by core–shell structured Fe3O4@COFs nanospheres and (f) after extraction on bare Fe3O4 nanospheres under optimum condition. Peak identity: 1, SDZ; 2, SMR; 3, SMZ; 4, SMX; 5, STZ; 6, SDM. Reproduced with permission from ref. 114. Copyright 2019 Elsevier B.V. |
Thereafter, to check the superiority of the Fe3O4@COF nanospheres, the extraction of six SAs were evaluated systematically using MSPE coupled with HPLC. In the extraction process, initially, the target analyte SAs were pre-treated via sample pre-treatment technique (MSPE) and further subjected to quantitative analysis via HPLC. The chromatograms of six SAs with extraction, without extraction and by using Fe3O4 nanospheres are shown in Fig. 13d–f, which illustrates the high extraction efficiency of core–shell Fe3O4@COF nanospheres. The results revealed that out of the six SAs, SMX and SDM with methoxy groups substituted on pyrimidine ring displayed higher extraction efficiency instead of methyl substitution. The reason stated that the methoxy group could form conjugation which lowered the basicity of pyrimidine ring, thereby enhancing the electrostatic and π–π interaction with porphyrin ring than that of methyl substitution. From Fig. 13f, it is observed that in comparison to Fe3O4@COF, bare Fe3O4 showed much lower peak area of SAs extraction. This is due to multiple interactions between COF layer and SAs. Also, Fe3O4@COF showed strong adsorption affinity for SAs due to their high surface area and porosity, which also leads to enhancement of extraction efficiency. The method presented a wide linear range from 1 to 500 ng mL−1. The LOD for six SAs were ranged from and 0.2–1 ng mL−1 with R2 higher than 0.99. Further, the established method was applied in real samples including milk, pork, chicken, lake water and shrimp for the detection of SAs. The MSPE-HPLC method showed excellent recoveries (65.3–107.3%) in environmental water and food with RSD ≤ 6.7. Hence, specific surface area, high stability, good porosity and large π-conjugated system endowed Fe3O4@COF nanospheres as an excellent sorbent for the analysis of SAs.
Likewise, Zhou and co-workers fabricated thiolated-β-cyclodextrin-functionalized MagCOFs for the extraction of trace SAs from meat samples (Fig. 14).115 The approach involved amino-modified MNPs as the support material. In this case, β-CD could form inclusion complexes via capturing targeted analytes into its cavity through host–guest relationship. It was prepared by direct solvothermal method by taking FeCl3 as the iron source and ((3-aminopropyl)triethoxysilane) (APTES) as –NH2 source (to facilitate the Schiff base reaction between COF monomers and magnetic core). After its formation, the monomers Tp and Bd were covalently grafted on the surface of Fe3O4-NH2 to form Fe3O4@COF. Further, Fe3O4@COF@Au was obtained by initial immobilization of AuCl4·4H2O on Fe3O4@COF by electrostatic interaction between amine group and AuCl4−, followed by reduction of Au(III) to Au NPs using NaBH4 as the reductant. Finally, β-CD functionalized COF (Fe3O4@COF@Au-β-CD) was formed by Au-S bonding between Fe3O4@COF@Au and thiolated-β-CD.
Fig. 14 (a) Schematic illustration for the synthesis for Fe3O4@COF@Au-β-CD and (b) the MSPE procedure for the determination of SAs in meat. Reproduced with permission from ref. 114 Copyright 2020 Springer Nature Publishing AG. |
The final material Fe3O4@COF@Au-β-CD (with COF thickness being 25 nm) was exploited for the extraction of nine SAs. The extraction of SAs increased due to hydrogen bonding between hydroxyl groups on the surface of MagCOF and amino groups of SAs. Additionally, the presence of π interaction between phenyl rings, uniform pore structure and the large specific surface area also enhances the extraction efficiency. Besides, hydrophilicity and polarity also played a vital role in extraction process. To check the applicability of this adsorbent, authors studied linearity, LOD, precision and RSDs under optimized conditions. It was found that the proposed method showed good linearity in the range of 2–100 μg kg−1 and the LODs were calculated to be 0.8–1.6 μg kg−1 (S/N = 3). Moreover, the authors performed extraction process at two kinetic models: pseudo-first-order and pseudo-second-order and it was found that pseudo-second-order kinetic was better fitted with the adsorption kinetics of SAs with R2 greater than 0.99. Admiringly, the proposed method was magnificently applied for quantification of SAs from real samples. The recoveries were ranged from 78.9 to 112.0%. The fabricated magnetic adsorbent furnished high extraction efficiency of trace SAs under mild conditions.
Considering the benefits of MagCOFs, Qian and co-workers fabricated Fe3O4@TpPa-1 via a two-step solvothermal reaction and investigated the efficacy of the material for the hydrophilic enrichment of N-glycopeptides from standard glycoproteins and human serum digests by Hydrophilic interaction chromatography (HILIC) (Fig. 15).119 To synthesize crystalline keto-enamine linked Fe3O4@TpPa-1, initially, Fe3O4 (of size 40 nm) were obtained by hydrothermal method. Subsequently, the monomers Tp and Pa were grafted over MNPs through in situ solvothermal reaction to acquire MagCOF. The highly ordered 2D topology with nitrogen rich frameworks and amino-terminals enhances the enrichment efficiency for N-glycopeptides. The TEM and SEM images (Fig. 15b and c) show sea-urchin type morphology of the adsorbent, which could provide increased specific surface area and available active sites which are highly advantageous for mass transfer and separation processes.
Fig. 15 Schematic illustration of the (a) synthesis of Fe3O4@TpPa-1, (b) SEM, (c) TEM image of Fe3O4@TpPa-1, MALDI-TOF MS spectra of human IgG digest (70 fmol μL−1) (d) direct analysis, (e) after enrichment by Fe3O4 and (f) after enrichment by Fe3O4@TpPa-1. Reproduced with permission from ref. 119. Copyright 2017 Royal Society of Chemistry. |
Further, the feasibility of Fe3O4@TpPa-1 was checked in the enrichment of N-glycopeptides using tryptic digests of a standard glycoprotein (human IgG). Fig. 15d–f represents that without enrichment, only six peaks of glycopeptides with lower intensities were observed. However, after enrichment with Fe3O4@TpPa-1, 37 glycopeptide peaks were analyzed with high MS signal intensities and increased S/N ratio which was higher than previously reported literature. Further the activity of bare MNPs was also tested: only 6 glycopeptide peaks were detected along with the detection sensitivity of Fe3O4@TpPa-1 at different concentrations. It was found that upon a decrease in concentration, the number of glycopeptides was decreased. Moreover, the selectivity and specificity test of Fe3O4@TpPa-1 was also evaluated using digest mixture of IgG and bovine serum albumin. Results indicated that Fe3O4@TpPa-1 showed fast, efficient and selective enrichment of N-glycopeptides. Inspired by the results, the authors also investigated the capability of Fe3O4@TpPa-1 in tryptic digests of human serum, which greatly showed identification of 228 glycopeptides corresponding to 114 glycoproteins within three independent replicates which is better than commercial HILIC. The LOD was found to be low (28 fmol) with recoveries of 94.3% and 86.3% for two deglycopeptides.
On a similar note, Deng et al. presented a promising approach for the enrichment of endogenous glycopeptides in human saliva by designing hydrophilic MagCOF (mCTpBd) as shown in Fig. 16.120 The mCTpBd with inherent hydrophilicity has been synthesized by the following procedure: first of all, Fe3O4 were synthesized by solvothermal method and to facilitate the growth of COF shell, MNPs were coated with a layer of silica via sol–gel approach. Thereafter, to enhance the interaction, amine groups were introduced by surface modification of the silica encapsulated MNPs using APTES (Fe3O4-NH2; 336 nm). Furthermore, Fe3O4-NH2 surface was pre-modified using a monomer, carboxyl-modified 1,3,5-triformylphloroglucinol, CTp via amidation reaction (Fe3O4-NH2-CTp), to boost the interaction among inorganic magnetic core and organic moieties. Finally, mCTpBd (398 nm; 31 nm COF thickness) was obtained by the reaction between Fe3O4-NH2-CTp and another monomer Bd through interface deposition method with reflux conditions under argon atmosphere. mTpBd was also synthesized in a similar manner.
Fig. 16 Synthetic route of mCTpBD and enrichment procedure of glycopeptides by mCTpBD. Reproduced with permission from ref. 120. Copyright 2020 American Chemical Society. |
In order to study the enrichment performance of mCTpBd for glycopeptides, it was first tested for HRP tryptic digest. It was observed that the introduction of mCTpBd greatly enhanced enrichment performance. Before enrichment, only a few of the glycopeptides were observed. Results showed that after enrichment with mTpBd and mCTpBd, the number of glycopeptide peaks were increased. But, enrichment performance of mCTpBd was vastly improved in comparison with mTpBd, revealing the enhanced hydrophilicity obtained from the carboxyl-modified monomer. Further, the adsorption capacity remained nearly intact even after continuous adsorption–desorption cycles. Inspired by the outstanding results of mCTpBd, it was also deployed for the enrichment of glycopeptides from biological samples (saliva of healthy people and patients with inflammatory bowel disease). Noteworthy, the magnetic adsorbent possessed excellent enrichment capacity in both the cases. Subsequently, mCTpBd with inherent hydrophilicity is a favourable candidate for the enrichment of endogenous glycopeptides.
Another kind of guanidyl-functionalized MagCOF has been synthesized by Wu et al. via post synthetic modification using stable precursors including 2,5-divinylterephthalaldehyde and TAPB.121 These two precursors were reacted along with Superparamagnetic iron oxide nanoparticles (SPIO) to form grafted COF, i.e. SPIO@COF. To provide NH2 functionality, cysteamine was introduced on SPIO@COF by thiol–ene “click” reaction to obtain SPIO@COF@NH2 nanospheres. As guanidyl is a group having efficient affinity for specific phosphopeptide enrichment, guanidinylation of SPIO@COF@NH2 nanospheres was carried out using 2-ethyl-2-thiopseudourea hydrobromide to form SPIO@COF-guanidyl nanospheres (20 nm COF thickness) (Fig. 17). The so-formed magnetic adsorbent was used for the selective enrichment of endogenous phosphopeptides from human saliva and analyzed by MALDI-TOF MS. Impressively, due to large surface area, abundant affinity groups, mesoporous structure and excellent magnetic response, SPIO@COF-guanidyl exhibited excellent performance for the selective enrichment of phosphopeptides.
Fig. 17 (a) Synthetic illustration of the SPIO@COF-guanidyl nanospheres and (b) workflow of the enrichment strategy for phosphopeptides by SPIO@COF-guanidyl nanospheres. Reproduced with permission from ref. 121 Copyright 2020 Elsevier B.V. |
Likewise, Jia et al. developed guanidyl-based magnetic ionic COFs (Fe3O4@iCOFs) using guanidyl as ionic ligand instead of post synthetic modifications.122 Fe3O4@iCOF was fabricated by immobilizing benzene-1,3,5-tris-carbaldehyde and 1,3-diaminoguanidino hydrochloride on the surface of MNPs (of size 150 nm)through hydrogen bond interactions (Fig. 18). The fabricated magnetic adsorbent was then utilized for selective enrichment of phosphopeptides. The reason behind phosphopeptides enrichment is electrostatic and hydrogen bonding interactions between phosphate and guanidyl groups. By combining with MALDI-TOF MS determinations, Fe3O4@iCOFs exhibited good enrichment capacity for phosphopeptides. The developed protocol offered several key advantages such as superparamagnetism, high sensitivity and selectivity along with recycling up to seven times.
Fig. 18 Synthetic scheme of Fe3O4@iCOFs for selective enrichment of phosphopeptides with Fe3O4@iCOFs. Reproduced with permission from ref. 122. Copyright 2020 Elsevier B.V. |
On a similar note, another magnetically recyclable core–shell structure featuring Ti4+ functionalized microporous COF was synthesized by Zhang et al. The synthesis of Fe3O4@SiO2@TpPa-Ti4+ (40 nm COF thickness) is depicted in Fig. 19a wherein MNPs were used as magnetic core and functionalized with silica layer via Stöber sol–gel approach.123 Surface modification of Fe3O4@SiO2 was carried out by introducing amine groups on its surface using APTES. The magnetically retrievable adsorbent could be easily recovered from the reaction mixture and hence, prevented the loss and separation time of adsorbent. Subsequently, Tp, a monomer of COF was immobilized on amino functionalized MNPs to form Fe3O4@SiO2-Tp. In addition, to obtain Fe3O4@SiO2-TpPa-NO2, reversible growth of microporous TpPa-NO2 was performed on Fe3O4@SiO2-Tp. Fe3O4@SiO2-TpPa-NO2 further underwent a reduction in the presence of NaBH4 to convert nitro groups into amino groups for the further phosphate-linking reaction. Also, during the reduction process the imine linkages of COFs were converted into secondary amines, which could provide good hydrophilicity to capture phosphopeptides. Finally, due to strong affinity between phosphates and titanium ions, titanium ions were chelated to phosphates. As shown in Fig. 19b, Fe3O4 nanoparticles displayed nearly spherical shape with the average particle size of 220 nm. Fig. 19c shows the TEM image of Fe3O4@SiO2 with dark MNP core coated by grey silica shell of ∼20 nm. This silica layer not only protect Fe3O4 from aggregation but also provides sites for the functionalization of amino groups which is necessary for the reversible assembly of covalent organic frameworks. Besides, after in situ Schiff-base condensation reaction, a porous covalent organic layer with thickness of 40 nm over Fe3O4@SiO2@TpPa-NO2 nanoparticles was observed (Fig. 19d). Further, TEM images of Fe3O4@SiO2@TpPa-Ti4+ and EDX-mapping image of Fe, Si and Ti showed uniform spherical morphology and smooth surface of the synthesized composites and reveals that Ti4+ groups were densely grafted into inner channels and surface of COFs (Fig. 19e and f).
Fig. 19 (a) Synthetic route of Fe3O4@SiO2@TpPa-Ti4+ nanoparticles, TEM images of (b) Fe3O4, (c) Fe3O4@SiO2, (d) Fe3O4@SiO2@TpPa-NO2, (e) Fe3O4@SiO2@TpPa-Ti4+, (f) elemental mapping of Fe3O4@SiO2@TpPa-Ti4+ (the first image without elemental labelling is high magnification TEM image), MALDI-TOF mass spectra of α-casein (g) before enrichment and (h) after enrichment with Fe3O4@SiO2@TpPa-Ti4+. Reproduced with permission from ref. 123 Copyright 2020 Royal Society of Chemistry. |
The as-synthesized magnetic adsorbent was utilized for selective enrichment of phosphopeptides from bio samples. In this case, tryptic standard phosphoprotein (α-casein) digests are used as model samples to evaluate the phosphopeptide enrichment performance of Fe3O4@SiO2@TpPa-Ti4+ composite. Fig. 19g and h demonstrates MALDI-TOF mass spectra of α-casein before enrichment and after enrichment with Fe3O4@SiO2@TpPa-Ti4+. The spectra suggested that only two phosphopeptide peaks (m/z = 1466.7 and 1927.7) were observed before enrichment at very low signal-to-noise ratio and after enrichment with magnetic adsorbent, thirty peaks of phosphopeptides were detected, indicating an excellent performance of so-formed magnetic adsorbent. The selectivity of Fe3O4@SiO2@TpPa-Ti4+ was also checked in presence of other samples. The proposed method gave high precision with low LOD, which could be attributed to abundant affinity sites. Also, Fe3O4@SiO2@TpPa-Ti4+ showed admirable performance in rat brain lysates with a high specificity of 91.8%.
In view of this, Salonen et al. performed extraction of OA and DTX-1 from sea-water in the presence of magnetically retrievable crystalline COF (mTpBd-Me2).75 To obtain mTpBd-Me2, a controllable simplified three-step procedure was carried out. Firstly, amino-functionalized MNPs were obtained by co-precipitation method by introducing dopamine as capping agent (Fe3O4@DOPA; 5 nm). Secondly, a monomer Tp was pre-functionalized on the surface of Fe3O4@DOPA (Fe3O4@DOPA-Tp); pre-grafting facilitates the nucleation and growth of COF shells around dopamine functionalized MNPs. Lastly, to grow mTpBd-Me2, another COF monomer, di-methyl benzidine (Bd-Me2) and Tp/o-tolidine in a 1:1.5 molar ratio was exposed on the pre-functionalized MNPs in the presence of acetic acid as catalyst (Fig. 20). Noteworthy, non-pre-grafted Fe3O4@DOPA led to amorphous COFs.
Fig. 20 The three-step synthesis of mTpBD-Me2. Reproduced with permission from ref. 75. Copyright 2019 Royal Society of Chemistry. |
The optimal concentration for the synthesis of mTpBd-Me2 was tested with the amount of Tp ranging from 0.005 to 0.4 mmol. Further, 0.1, 0.2 and 0.4 mmol yielded crystalline composites such as 0.1-mTpBd-Me2, 0.2-mTpBd-Me2 and 0.4-mTpBd-Me2. In addition, 0.2-mTpBd-Me2 was selected for the extraction of OA and DTX-1 due to their high organic content and stability up to 380 °C. The kinetic studies showed fast adsorption due to presence of large surface of the nanocomposite. Moreover, the adsorption isotherm for both the biotoxins displayed n > 1, demonstrating favourable adsorption. Furthermore, a good adsorption capacity of the sorbent was found to be 26.363 mg0.219 g−1 L0.781 and 22.508 mg0.181 g−1 L0.819 for OA and DTX-1, respectively, which was indicated by KF (indicator of adsorption capacity in Freundlich theory) value. Additionally, the maximum adsorption capacity was calculated to be 812 mg g−1 for OA and 830 mg g−1 for DTX-1, which was three-fold higher for OA as compared to bulk TpBd-Me2. Also, mTpBd-Me2 exhibited higher calculated adsorption kinetics, i.e., ∼500-fold increase for OA and ∼300-fold increase for DTX-1 as compared with literature precedents. This increase can be attributed to the ordered pore structure of MagCOFs which allows higher diffusion rates for bio-toxins instead of non-magnetic bulk COFs which are difficult to separate from sample matrix. Besides, the recyclability efficiency of the adsorbent was also examined and was found that the adsorbent could be reused for at least five consecutive cycles. Consequently, mTpBd-Me2 had good potential for rapid extraction of marine biotoxins from sea water. The adsorption and concentration of other pollutants such as pesticides and detoxification of other bio-toxins can also be studied using mTpBd-Me2 as adsorbent. Moreover, routine monitoring of OA and DTX-1 in sea water is essential to avoid shellfish contamination.
Fig. 21 Schematic diagram for the synthesis of M-COF-SH. Reproduced with permission from ref. 131. Copyright 2020 Elsevier B.V. |
Subsequently, three M-DAPS-COFs with three different molar ratios (0%, 50% and 100%) of DAPS were synthesized. Remarkably, amongst all, M-DAPS50-COF was obtained in high yield (∼95%). It contains densely distributed thioether side chains as the Hg2+ receptor due to strong soft-soft interaction between sulfide and mercury. Impressively, Mag-COF-SH showed maximum adsorption capacity of Hg2+ (383 mg g−1) which can be attributed to the abundant thiol functional groups and ultra-porous structure of the framework. The selectivity towards Hg2+ detection was also checked in presence of other competitive metal ions and satisfactory results were obtained. Moreover, resulting composite exhibited rapid kinetics, i.e., adsorption equilibrium can be achieved within 10 min, which was attributed to high specific surface area of MagCOF composite and strong affinity between thiol (–SH) moieties and Hg2+. Additionally, to evaluate the disconnection of disulfide linkages, integration of MNPs over COF and formation of imine bonds, XPS, XRD and FT-IR spectra were studied, which illustrates satisfactory results. Besides, Mag-COF-SH could be reused up to five adsorption cycles which proposed its use in large scale metal sensing and removal applications.
Chromium is extensively used in various industries including electroplating, leather tanning, metal finishing, pigment synthesis, petroleum refining, etc. Two stable forms of chromium exist in environment, trivalent Cr3+ and hexavalent Cr6+. However, Cr6+ is considered as more hazardous due to its high mobility and solubility in water and soil. Owing to its greater penetration, it can severely affect central nervous system and is a classified carcinogen due to its oxidizing nature.132 Besides chromium, BPA is also a known pollutant which was discussed thoroughly in the previous section.
In view of this, Hu et al. performed removal of Cr6+ and BPA from aqueous solution using magnetically retrievable COF (Fe3O4@COF; TpPa-1 thickness being 10 nm) with β-ketoenamine linkage under solvothermal reaction conditions (Fig. 22a).133 The as-synthesized magnetic adsorbent reflected numerous advantages such as simple preparation method, excellent adsorption performance, high stability and good recoverability (19.5 emu g−1). TEM images of TpPa-1 and Fe3O4@TpPa-1 illustrate sea-urchin type and spherical morphology with an average diameter of ∼80–100 nm, respectively (Fig. 22b and c). The effect of pH, ionic strength and adsorption isotherms are the key factors in the extraction process. The thermodynamic as well as kinetic studies validate to the pseudo-second-order and Langmuir isotherm indicating spontaneous, endothermic and chemisorption process. The mechanism of BPA extraction follows π–π stacking interaction, hydrogen-bond and porosity induced by hydrophobicity. Moreover, for Cr6+ adsorption, firstly anionic Cr6+ was combined with the surface protonated functional groups of TpPa-1. Secondly, Cr6+ was reduced to Cr3+ with the aid of adjacent electron donor groups. Finally, reduced Cr3+ was returned into solution due to electronic repulsion. The adsorption capacities for Cr6+ and BPA were measured to be 245.45 mg g−1 and 1220.97 mg g−1, respectively. Additionally, magnetic adsorbent was reused for five adsorption–desorption cycles. Nevertheless, there exists certain fundamental aspects which needs to be focused. In our view, influence of different coexisting anions in adsorption behaviours of Cr3+ and Cr6+ should be studied to improve the effectiveness of the process. Further, present strategies mainly target the batch extraction, however, continual removal of Cr6+ from industrial effluents is more useful as effluents mainly originate from industries involved in production of large amounts of waste.
Fig. 22 (a) Synthesis process of core–shell structured Fe3O4@TpPa-1, TEM image of (b) TpPa-1 and (c) Fe3O4@TpPa-1. Reproduced with permission from ref. 133. Copyright 2020 Elsevier B.V. |
Fig. 23 Synthesis and application of MagCOFs@MIPs@CDs as fluorescent sensor. Reproduced with permission from ref. 135. Copyright 2020 Elsevier B.V. |
The fabricated MagCOF@MIP@CD was further utilized as a fluorescent sensor for environmental pollutant TNP. The maximum excitation and emission wavelength were recorded to be 370 nm and 470 nm, respectively. MagCOF@MIP@CD without TNP exhibited strong fluorescence signal which was quenched in presence of TNP. Amongst various competitive compounds of TNPs and metal ions, best selectivity was obtained for TNP due to the effective π–π interaction and hydrophobic effect between TNP with MagCOF@MIP@CD. Hence, MagCOF@MIP@CD not only provided excellent magnetism and good fluorescence but also exhibited good sensitivity with high imprinting factor (8.4) and shorter detection time (within 1 min). Delightedly, good recoveries (88.7% to 103.4%) were obtained when the fluorescent sensor was applied in real samples. Moreover, recyclability of the sensor up to eight consecutive runs also imparted green credentials for their use at large scale.
Along with nitroaromatic explosives, selective and sensitive detection of endocrine disruptor, PAHs and many more organic pollutants have raised incredible attention due to their adverse effects on aquatic ecosystems, humans and environmental health (Fig. 24).136 Also, cigarette smoke is composed of various chemicals including gaseous nicotine and tar which have carcinogenic effect on human health. Inhaling such toxic chemicals, Bap and phenols, may cause cancer and many other diseases.137,138 Therefore, adsorption and removal of these organic pollutants are of great necessity. To fulfil current needs, Zhang et al. synthesized novel porous aromatic framework (PAF) decorated MNPs, PAF-6 MNPs, using cyanuric chloride for triangular planar basis and piperazine as linker unit via one-step polymerization process as shown in Fig. 25.139 Zhang developed this sample pre-treatment method by coupling of MSPE with HPLC-UV for the adsorption of TNP, 3-nitrochlorobenzene, BPA, naphthalene and naphthol from well-water, tap-water, waste water and yellow river water.
Fig. 25 (a) Preparation procedure of core–shell microspheres (PAF-6 MNPs), (b) TEM image of PAF-6 MNPs and (c) effect of PAF-6 MNPs levels on the removal efficiency of phenolic compounds from cigarette smoke and (d) effect of PAF-6 MNPs dosage on the removal efficiency of Bap from cigarette smoke. Reproduced with permission from ref. 139. Copyright 2018 Elsevier B.V. |
The presence of aromatic units and nitrogen atoms provides them multiple recognition sites. The fabricated Porous aromatic framework-6 (PAF-6) MNPs showed remarkable adsorption capability due to presence of π–π interactions, hydrogen-bond interactions and inclusion complexation. TEM image of PAF-6 MNPs showed spherical core–shell structure with narrow size distribution (Fig. 25b). Moreover, PAF-6 MNPs were also used to identify toxicants present in cigarette smoke such as phenolic compounds (o,m,p-cresol, phenol, pyrocatechol, resorcinol and hydroquinone), Bap and tar. The results showed that upon increasing the amount of PAF-6 MNPs from 5 mg to 20 mg, the removal efficiencies increased rapidly (Fig. 25c and d). The method showed maximum adsorption capacity (166.85 mg g−1), good linearity for different organic pollutants in the range of 0.01–12 μg mL−1 and the R2 was more than 0.97; the LODs were between 0.083 and 5.020 according to the three-fold signal to noise ratio. The extraction efficiency of the method was in between 84.0% and 96.0% with reusability of at least six cycles. These magnetic porous composites exhibited high stability, desirable durability and enhanced magnetic separation. The results proved that PAF-6 MNPs displayed outstanding adsorption performance for diverse multi target analytes, nitrosamines, heavy metal ions and other toxic compounds.
Fig. 26 Schematic diagram for (a) magnetization of COF-(TpBD), (b) application of COF-(TpBD)/Fe3O4 as absorbent for MSPE and detection of PAEs. Reproduced with ref. 142, Copyright 2020 Elsevier B.V. (c) Synthesis of Fe3O4@PDA@TbBd. |
Similarly, Liang and co-workers fabricated MagCOFs by Schiff base condensation reaction of two monomers Tb and Bd on PDA functionalized Fe3O4 (Fig. 26c).143 In this case, PDA was used as a hydrophilic middle layer which displayed excellent water dispersibility and good biocompatibility. The synthesized adsorbent exhibited several advantages including high surface area, large number of active sites for PAEs detection (via π–π and hydrophobic interactions), easy separability and high aqueous dispersibility. The fabricated magnetic adsorbent was further deployed for recognition of nine PAEs from a human plasma sample. Favourably, Fe3O4@PDA@TbBd unveiled great potential in PAEs detection with wide linearity (50–8000 ng mL−1) and low LOD (0.0025–0.01 ng mL−1). The proposed strategy showed good recovery (92.3–98.9%) and a small RSD value (for intra-day <4.6% and for inter-day <6.8%). To check the superiority of the adsorbent it was applied in real sample analysis and favourable results were obtained. Besides, the adsorbent was magnetically recovered and used repeatedly for five cycles.
Recently, Rafiee and co-workers fabricated a melamine-rich magnetic covalent organic polymer (MCOP) for the removal of AO and RB.147Fig. 27a depicts the fabrication of the MCOP wherein MNPs (of sizes 20–50 nm) were synthesized by solvothermal technique. Surface modification of MNPs using glucose and polyacrylonitrile provided carboxylate units which ease the COP coverage easily onto Fe3O4. The final adsorbent (Fe3O4/C-COP) was formed by Schiff base condensation reaction between TPA and melamine on the surface of modified MNPs. Fig. 27b represents the mechanistic pathway for the removal of AO and RB. The presence of free lone pair electron in various imine groups present on Fe3O4/C-COP could electrostatically interact with cationic RB and AO, which enhanced the adsorption behaviour. Also, due to the planar structure of the dye it can be readily adsorbed on the adsorbent through hydrogen-bonding and van der Waals forces. Brunauer–Emmett–Teller (BET) surface area and Barrett–Joyner–Halenda (BJH) pore-size analyses confirmed the cavity encapsulation. The surface area and pore volume of Fe3O4/C-COP before and after adsorption was determined by BET analysis (Fig. 27c). The surface area and pore-volume before adsorption was calculated to be 150.51 m2 g−1 and 0.4125 cm3 g−1, respectively whereas after adsorption of AO and RB both surface area (38.89 m2 g−1) and pore-volume (0.2191 cm3 g−1) decreased. The decrease in values was due to encapsulation of AO and RB in the cavity. The authors also compared the results with previously reported adsorbents, which revealed better results in terms of mass (12 mg) and contact time (4 min). The maximum adsorption capacity for AO and RB were 107.11 and 131.23 mg g−1, respectively. The higher maximum adsorption capacity value for RB is attributed to the π–π interactions mechanism between RB and the material.
Fig. 27 (a) Schematic representation for the preparation of Fe3O4/C-COP, (b) proposed adsorption mechanism of AO/RB onto Fe3O4/C-COP and (c) VSM curves of Fe3O4 and Fe3O4/C-COP before and after AO and RB adsorption, (d) regeneration studies of magnetic Fe3O4/C-COP using ethanol and (e) N2 adsorption/desorption isotherm of Fe3O4/C-COP before (a) and after (b) AO and RB adsorption Reproduced with permission from ref. 147. Copyright 2020 American Chemical Society. |
From VSM analysis, the saturation magnetization value for Fe3O4/C-COP was observed to be 37.5 emu g−1 which is lower than the magnetization of bare Fe3O4 (81.5 emu g−1). Fig. 27d shows that Ms value of Fe3O4/C-COP after six cycles was found to be lower after AO and RB adsorption than the fresh Fe3O4/C-COP. This reduction in the saturation magnetization can be attributed to the fact that with the addition of AO and RB to Fe3O4/C-COP the surface magnetic anisotropy of magnetite changes which leads to an increase in surface spin disorientation. This results in the decrease of magnetic moment of the adsorbent and hence decrease in Ms value of Fe3O4/C-COP. Besides, due to simple magnetic recoverability, the adsorbent was reused for nine consecutive cycles.
In this regard, Gao and co-workers fabricated core–shell structured MagCOFs for the efficient extraction of six FQs (ciprofloxacin, enrofloxacin, lomefloxacin, gatifloxacin, levofloxacin and pefloxacin) from pork, milk and human plasma through MSPE coupled HPLC technique (Fig. 28a).158 The MagCOF was synthesized by immobilizing 4,4′′-diamino-p-terphenyl and 1,3,5-tris(p-formylphenyl) benzene onto Fe3O4 by Schiff base condensation reaction. The new magnetic adsorbent exhibited low density, high surface area, excellent porosity, high thermal stability and offered effortless magnetic separability. Moreover, VSM studies revealed that Fe3O4@COFs display excellent magnetization (36 emu g−1) (Fig. 28b). To check the feasibility of MagCOF, adsorption kinetics and isotherms were obtained. Fig. 28c depicts the saturation adsorption capacities of six FQs i.e., as the concentration of FQ in the solution increases, adsorption of FQ on Fe3O4@COFs increases whilst Fig. 28d demonstrates that adsorption capacities were gradually increased in the initial 30 min and after 30 min adsorption kinetic curves are flat. These results suggest that adsorption equilibria was achieved in 30 min. Furthermore, from adsorption isotherms it was noted that Freundlich isotherm was better fitted in FQs adsorption, indicating that the adsorption process is not caused by monolayer, but by various interactions. The adsorption mechanism of MagCOF to FQs was mainly attributed to hydrogen bonding and π–π interaction between phenyl rings. Further, under optimized conditions (sorbents dosage, extraction time, pH of samples solution, ionic strength, etc.) analytical performance was investigated. The MSPE coupled HPLC analysis presented wide linear range (2.5–1500 ng g−1), low LOD (0.5 ng g−1) with R2 > 0.9996. The method showed good recoveries (78.7–103.5%) in milk, pork and human plasma/actual samples with RSDs ranging from 1.5 to 4.3% for intra-day and 2.9% to 6.2% for inter-day. Besides, Fe3O4@COFs could be reused for ten adsorption–desorption cycles.
Fig. 28 (a) Synthesis and application of Fe3O4@COFs, (b) VSM studies of Fe3O4, (c) adsorption isotherms of six FQs on Fe3O4@COFs and (d) adsorption kinetics of six FQs on Fe3O4@COFs. Reproduced with permission from ref. 158 Copyright 2019 Springer Nature Publishing AG. |
Similarly, Li et al. synthesized sulfonate-functionalized MagCOF for the effective extraction of FQs in food samples through MSPE-HPLC-MS/MS method (Fig. 29).154 For the preparation, firstly Fe3O4 NPs were modified by Schiff base reaction between Tp and Bd. Further, Fe3O4@TpBd-Au was fabricated by loading gold nanoparticles on Fe3O4@TpBd. Furthermore, Fe3O4@TpBd-Au was functionalized by immobilization of sodium 3-mercaptopropanesulphonate via Au–S bond formation. The adsorption of FQs is attributed to the strong π–π stacking, hydrogen bonding and electrostatic interactions. The proposed method showed linearity with excellent R2 value (≥0.9989) and lower LOD (0.1–1.0 μg kg−1). Moreover, the method displayed satisfactory recoveries (82–110.2%) in food stuffs with lower RSDs. The as-synthesized magnetic adsorbent showed superior adsorption ability and magnificent chemical stability. Adsorption performance and structural parameters of variety of COFs have been listed in Table 2.
Fig. 29 Schematic fabrication process of Fe3O4@COF(TpBD)@Au-MPS and the MSPE procedure for the determination of FQs. Reproduced with permission from ref. 154. Copyright 2020 Elsevier B.V. |
MagCOF | Adsorption time (min) | Desorption time (min) | Adsorption dosage (mg) | Elution solvent | Surface area (m2 g−1) | Pore volume (cm3 g−1) | Pore size | Ref. |
---|---|---|---|---|---|---|---|---|
Fe3O4@COF | 30 | 3 | 40 | Methanol | 166.5 | 0.26 | n.d. | 148 |
NiFe2O4@COFs | 5 | n.d. | 10 | Acetonitrile:methanol | 169.7 | 0.276 | n.d. | 159 |
Fe3O4@TpBd | 5 | 1 | n.d. | Ethanol | 272.6 | 0.457 | 1.7 nm | 67 |
Fe3O4@COF | 10 | 2 | 20 | i-Propanol | 181.36 | 0.45 | 3.6 nm | 70 |
Fe3O4@COFs-Apt | 30 | n.d. | 30 | Hexane | 185 | n.d. | n.d. | 36 |
Magnetic TpPa-1 | n.d. | n.d. | 5 | Acetonitrile | 247.8 | 0.40 | 0.4–2.0 nm | 71 |
COF-LZU1@PEI@Fe3O4 | 30 | 3 | 5 | Acetonitrile | n.d. | n.d. | n.d. | 160 |
MOPs | 20 | 10 | 5 | Ethyl acetate | 378 | n.d. | n.d. | |
Mag-COF-2 | 20 | n.d. | 0.1 | Methanol | 334.9 | 0.32 | 3.9 nm | 149 |
MagCOF | 50-DCF 80-SMT | n.d. | 10 | Acetonitrile | 2245 | n.d. | 2.5 nm | 108 |
Mag-COF-1 | 60 min | 5 | 5 | Acetonitrile | n.d. | n.d. | 41 | |
Fe3O4@COF | 20 | 2 | 10 | Acetonitrile | 30.6 | 0.187 | 2–5 nm | 114 |
Fe3O4@COF@Au-β-CD | 30 | 10 | 20 | Acetonitrile-acetic acid | n.d. | n.d. | n.d. | 150 |
Fe3O4@TpPa-1 | 30 | 10 | 0.02 | Acetonitrile-H2O-TFA | 186 | 0.17 | 3.6 nm | 119 |
mCTpBd | 30 | 30 | 0.2 | Acetonitrile-H2O-TFA | 120.41 | n.d. | 1.3 nm | 120 |
SPIO@COF-guanidyl | 30 | 10 | 10 | Acetonitrile-H2O-TFA | 149.75 | n.d. | 3.2 nm | 121 |
Fe3O4@iCOFs | 30 | 15 | 5 | Acetonitrile-H2O | 7 | n.d. | n.d. | 122 |
Fe3O4@SiO2@TpPa-Ti4+ | 30 | 10 | 1 | Acetonitrile-TFA | 128 | n.d. | 1.4 nm | 123 |
mTpBd-Me2 | 60 | 4 h | n.d. | 2-Propanol | 538 | 0.40 | 1.1 nm | 152 |
M-DAPS-COF-SH | 10 | n.d. | 5 | HCl and thiourea | 181.5 | 0.24 | n.d. | 131 |
Fe3O4@COF(TpPa-1) | 10-BPA 100-Cr | n.d. | 5 | Ethanol | 485.2 | 0.34 | 2 nm | 153 |
MagCOF@MIP@CD | 30 | 2 | 0.5 | Methanol:acetic acid | 137.34 | n.d. | 4.72 nm | 151 |
PAF-6 MNPs | 5 | 5 | 60 | Acetonitrile | 120.2 | n.d. | 2–5 nm | 161 |
COF-(TpBd)/Fe3O4 | 30 | 15 | 30 | Methanol | n.d. | n.d. | n.d. | 142 |
Fe3O4/C-COP | 2 | 4 | 12 | Ethanol | 150.51 | 0.4125 | n.d. | 147 |
Fe3O4@COFs | 60 | 20 | 14 | Methanol | 124 | 0.386 | 3.1 nm | 158 |
Fe3O4@COF(TpBD)@Au-MPS | 30 | 25 | 20 | Formic acid:methanol | 70.14 | 0.15 | n.d. | 154 |
Fe3O4@TbBd | 30 | 2 | 20 | Acetonitrile | 202.18 | 0.65 | 2.8 nm | 155 |
Fig. 30 (a) Preparation of Fe3O4@TbBd nanobeads, (b) MSPE process for estrogens in urine samples, TEM images of (c) bare Fe3O4 NPs and (d) Fe3O4@TbBd nanobeads. Reproduced with permission from ref. 155. Copyright 2018 Elsevier B.V. |
Magnetic materials | Linear range (ng mL−1) | Limit of detection (ng mL−1) | Sample | Extraction time (min) | Recoveries (%) | Ref. |
---|---|---|---|---|---|---|
Endocrine disrupting chemicals | ||||||
Fe3O4@MIP | 0.5–100 | 0.1–0.3 | Canned orange/milk | 3 | 72–113 | 164 |
magG@PDA@Zr-MOF | 50–20000 | 0.1–1 | Water | 20 | 64.8–92.8 | 165 |
Fe3O4@C | 0.01–100 | 0.017–0.15 | Tap water | 20 | 47.9–119 | 166 |
Fe3O4@rGO | 2.5–100 | 1.23 | Tap water/river water/waste water | n.d. | 96.3–112.6 | 167 |
Fe3O4@COFs | 0.5–1000 | 0.08–0.21 | Tea drinks | 30 | 81.3–118.0 | 168 |
Ni@Fe2O4@COF | 0.1–200 | 0.019–0.096 | Tap/barrelled/river water; activated beverage; human urine/serum sample | 5 | 83.4–106.2 | 159 |
Fe3O4@COFs | 0.1–50 | 0.001–0.078 | Human serum | 10 | 93.0–107.8 | 70 |
Persistent organic pollutants | ||||||
Graphene/Fe3O4 composite | 0.03–80 | 0.009–0.020 | Water | 4 | 83–107 | 169 |
Fe3O4@ZIF-8 | 1.0–100 | 0.08–0.24 | Water | 8 | 85.6–103.6 | 170 |
Magnetic MIL-100(Fe) | 0.5–500 | 0.032–2.11 | Water | 10 | 81.4–126.9 | 171 |
PFu/Fe3O4 | 0.02–200 | 0.005–0.02 | Urine samples | 15 | 93.2–99.2 | 172 |
Magnetic TpPa-1 | 0.002–0.2 | 0.00024–0.00101 | Water | n.d. | 73–110 | 71 |
Sulfonamides Extraction | ||||||
CoFe2O4-graphene nanocomposite | 20–50000 | 1.59 | Milk | 20 | 62.0–104.3 | 173 |
Graphene-Fe3O4 nanoparticles | 5–200 | 0.89–2.31 | Milk | 15 | 62.7–104.8 | 174 |
Fe3O4@GO | 2.0–100 | 0.02–0.13 | Milk | 5 | 73.4–97.4 | |
Polypyrrole/SiO2/Fe3O4 nanoparticles | 0.30–200 | 0.30–1 | Water | 20 | 86.7–99.7 | 175 |
Fe3O4@COFs | 1–500 | 0.2–1.0 | Water, milk, pork, chicken, shrimp | 20 | 65.3–107.3 | 114 |
Fe3O4@COF@Au-β-CD | 2–100 | 0.8–1.6 | Meat | 30 | 78.9–112.0 | 150 |
Metal ion extraction | ||||||
Magnetic materials | Maximum adsorption capacity (mg g−1) | |||||
Fe3O4@SiO2 | 148.8 | 176 | ||||
γ-Fe2O3@CTF-1 | 165.8 | 177 | ||||
MPTS-mesoporous Fe3O4/C@SiO2 | 118.6 | 178 | ||||
Fe3O4@SiO2-NH2 | 27.2 | 179 | ||||
M-DAPS50-COF-SH | 383 | 131 | ||||
Fe3O4@TpPa-1 | 246.45 | 153 |
However, despite the promising results, the full potential of the MagCOFs composites in certain areas of concerns still need further improvement Besides, not only the extraction of EDCs, POPs, PAHs and metal ions, extraction of microorganisms will also need to be studied to fully open up their application as versatile adsorbent. Moreover, systematic and continuous efforts are required for better designing and large-scale applications of MagCOFs in various fields. In the next step, it is also necessary to gain insights about the toxicity of the nanomaterials for their long-term use. Another important point to consider is the better understanding of adsorption–desorption mechanism i.e. to avoid the use of non-green and costly solvents. Other aspect, which is of utmost importance is the synthetic cost and efficiency of the MagCOF composites. The use of high cost monomers to synthesize COFs materials is not economical. Therefore, to enhance manufacturing efficiency by reducing the monomers cost through incorporating cost-effective functional groups is a significant topic from future perspective. Also, large-scale magnetic separation of EDCs, marine bio-toxins, PPCPs, POPs, etc. from large amount of crude culture media at standard conditions is still required. In terms of extraction applications, MagCOFs materials have shown enhanced performance but the use of MagCOFs in catalysis and other applications is still in its infancy. Therefore, there is need to expand the scope of application. Also, due to presence of stable π–π stacking between COF layers, it can greatly improve the photocatalytic reactions. But it is believed that post-synthetic modification at the pore will provide opportunities for incorporation of specific active sites for catalysis.
Despite these above-mentioned challenges, undoubtedly, the progress in recent years have predicted well for the bright future of this new type of porous materials and we sincerely hope that the present review will significantly contribute in facilitating that development in near future.
This journal is © The Royal Society of Chemistry 2022 |