Shihao Xin,
Xinxin Peng*,
Yao Zhang,
Aiguo Zheng,
Changjiu Xia,
Min Lin,
Bin Zhu,
Zuoxin Huang and
Xingtian Shu
State Key Laboratory of Catalytic Materials and Reaction Engineering, Research Institute of Petroleum Processing, SINOPEC, 100083, Beijing, PR China. E-mail: pengxx.ripp@sinopec.com
First published on 10th February 2022
A tungsten containing catalyst catalyzed oxidative cleavage of methyl oleate (MO) by employing H2O2 as an oxidant and is known as an efficient approach for preparing high value-added chemicals, however, the tungsten leaching problem remains unresolved. In this work, a binary catalyst consisting of tungsten oxide (WO3) and spongy titanosilicate (STS) zeolite is proposed for MO oxidative cleavage. The function of STS in this catalyst is investigated. On the one hand, STS converts MO to 9,10-epoxystearate (MES), which further forms nonyl aldehyde (NA) and methyl azelaaldehydate (MAA) with the catalysis of WO3. In this way, MO oxidation and hydrolysis that generates unwanted diol product 9,10-dihydroxystearate (MDS) decreases obviously. On the other hand, STS decomposes peroxide and promotes the conversion of soluble peroxotungstate to insoluble polytungstate. Meanwhile, these tungsten species are allowed to precipitate on its surface instead of remaining in the liquid phase owing to its relative large specific area. Therefore, tungsten leaching can be reduced from 37.0% to 1.2%. Due to the cooperation of WO3 and STS, 94.4% MO conversion and oxidative cleavage product selectivity of 63.1% are achieved, and the WO3–STS binary catalyst maintains excellent catalytic performance for 8 recycling reactions.
Common oxidants such as potassium permanganate and ozone can be used for oxidative cleavage reaction of UFAE.6–9 However, the toxicity and potential harm to humans limit their application. Some researchers turned to use hydrogen peroxide (H2O2) as an oxidant for this reaction10–12 as H2O2 is environmentally benign and produces water as the only by-product. Some transition metal containing catalysts,13–16 such as H2WO4@Al-MCM-41,12 BaFeO3−δ,17,18 Ru(OH)x/γ-Al2O319 and VO@TiO220 have been proved efficient in catalyzing this reaction with H2O2 as oxidant. Among them, tungsten containing catalysts such as tungsten oxide (WO3), WO3 nanoparticles,24 tungstic acid,25 tungstates and supported WO326–30 have shown the best catalytic performance.4,21–23
Although effective in catalytic oxidative cleavage of UFAE, tungsten containing catalyst suffers from active center leaching problem, and thus limits its large scale application. Take catalytic oxidative cleavage of MO by WO3 and H2O2 for example, the reason for tungsten leaching has already been illuminated.31–33 WO3 firstly reacts with H2O2 to form the active peroxotungstate species, which are soluble in the reaction system. Then, peroxotungstate converts MO into oxidation products and itself turns into insoluble polytungstate species. This compound could be regenerated into active peroxotungstate through reacting with H2O2, so the reaction cycle can be continued. After finishing the reaction, residual H2O2 would still react with polytungstate, and part of soluble tungsten species would remain in the reaction solution which leads to the loss of tungsten and lower the reusability of the catalyst. Therefore, in order to improve the performance and reusability of WO3 catalyst, it is important to reduce the residual soluble tungsten species within the reaction system.
In this work, we report a robust binary catalyst consisting of WO3 and spongy titanosilicate (STS) zeolite for this reaction. It is found that the addition of STS would enhance the epoxidation of MO, accelerating the consumption of H2O2 which promoted the precipitation of tungsten species. Additionally, the relatively large specific surface area of STS facilitates the capture of precipitated tungsten species and thus improves the reusability of the catalyst. Compared with WO3 catalyst, WO3–STS binary catalyst demonstrated improved catalytic performance (94.4% MO conversion and >63% oxidative cleavage products selectivity) and excellent reusability (8 cycles without significant loss in catalytic performance).
Samples | Relative crystallinity (%) | Ti/Si | SBET (m2 g−1) | Sext (m2 g−1) | Smicro (m2 g−1) | Vmeso (cm3 g−1) |
---|---|---|---|---|---|---|
TS-1 | 100 | 0.0355 | 440 | 48 | 392 | 0.104 |
STS | 78 | 0.0350 | 528 | 129 | 206 | 0.143 |
Nitrogen adsorption–desorption isotherm as well as BET and BJH methods were employed to investigate the texture properties of TS-1 and STS (Table 1 and Fig. 2a). Both two samples show type-IV isotherms with H4 type hysteresis loops (Fig. 2a), suggesting the formation of mesopores and multi-layer adsorption of N2. The relatively large hysteresis loop of STS which is mainly located at medium pressure zone (0.45 < p/p0 < 0.9) indicates a uniform distribution of mesoporous structure. Texture properties of TS-1 and STS (Table 1) confirms the existence of mesopores. Moreover, STS shows a narrow pore size distribution at around 4 nm, which is absent from TS-1 (Fig. 2b). It could be due to the effective pore-making effect of PHATMS reagent.
Fig. 2 (a) Nitrogen adsorption–desorption isotherms of TS-1 and STS, (b) pore size distribution of TS-1 and STS. |
SEM and TEM images of TS-1 and STS zeolites are shown in Fig. 3. Both TS-1 and STS present “raspberry-like” spherical morphology with relative smooth surface. The average particle size is about 300 to 400 nm. TEM image shows solid structure of TS-1, while STS is spongy-like morphology with intracrystalline mesoporosity owing to the aggregation of small particles. It is also found that due to the small particles of STS, the intensity of XRD is lowered down and its relative crystallinity is much lower than that of TS-1.
The XRD pattern of WO3 displayed in Fig. 1 clearly shows monoclinic crystal phase (JCPDS no. 43-1035). Then we prepared WO3-STS sample by mechanical mixing WO3 and STS in a mortar with mass ratio of 15:100 and characterized it by XRD. The result in Fig. 1 shows that the peak intensity of both WO3 and STS are decreased. Compared with WO3, the characteristic peaks of STS is more difficult to be recognized.
Entry | Catalyst | Conversion (%) | Selectivity (%) | Tungsten leaching (%) | |||||
---|---|---|---|---|---|---|---|---|---|
NA | PA | MAA | MHA | MES | MDS | ||||
a n(MO):n(H2O2):n(t-BuOH) = 1:2.5:20, m(catalyst):m(MO) = 1:10, temperature 80 °C, reaction time 4 h. | |||||||||
1 | — | 0 | 0 | 0 | 0 | 0 | 0 | 0 | — |
2 | SS | 0 | 0 | 0 | 0 | 0 | 0 | 0 | — |
3 | TS-1 | 9.8 | 0 | 0 | 0 | 0 | 100.0 | — | |
4 | STS | 30.8 | 5.3 | 2.5 | 5.5 | 2.0 | 69.5 | 15.2 | — |
5 | WO3 | 91.8 | 14.2 | 1.1 | 13.1 | 0.9 | 20.2 | 50.5 | 37.0 |
6 | WO3–TS-1 | 76.5 | 19.6 | 0 | 20.9 | 0 | 12.3 | 47.2 | 25.0 |
7 | WO3–SS | 90.1 | 13.2 | 0.7 | 12.6 | 0.5 | 21.7 | 51.3 | 42.0 |
8 | WO3–STS | 91.9 | 28.5 | 2.6 | 29.7 | 2.3 | 6.3 | 30.6 | 1.2 |
When we use mechanical mixture of WO3 and TS-1 as catalyst, MO conversion is much higher than Ts-1 but lower than WO3. Compared with products distribution of WO3, the selectivity of MES decreased to 12.3%, both NA and MAA selectivity increased and the MDS selectivity also decreased slightly. It suggests that the products distribution could be mediated by combining WO3 and TS-1. However, the WO3 leaching is still up to 25.0% and is unacceptable for a sustainable process. The performance of WO3–SS is basically the same with WO3 (Table 2, entry 5 and 7) as well as the tungsten leaching rate, suggesting that SS is ineffective for the MO oxidative cleavage reaction. Further, we used the binary WO3–STS as catalyst for MO oxidative cleavage reaction. The results showed MO conversion is higher than WO3 (91.9%). In contrast with WO3 and WO3-TS-1, the selectivity of NA and MAA is much higher and both MES and MDS decreases obviously. Among all catalysts, the highest MO conversion and total selectivity of oxidative cleavage products (NA, PA, MAA and MHA, 63.1%) are achieved by WO3–STS. More importantly, tungsten leaching of WO3–STS is reduced from 37.0% to 1.2%. The increased catalytic activity, enhanced oxidative cleavage products selectivity and suppressed tungsten leaching suggest synergistic effect from the combination of WO3 and STS. The dependence of catalyst amount on the MO oxidative cleavage reaction is investigate and provided in ESI Table S1.† The results also confirms both W and Ti are essential for this reaction.
While for WO3–STS, the story is totally different. After eight reaction cycles, the catalyst shows almost no loss of catalytic activity and oxidative cleavage products selectivity, the MO conversion even increases to 94.4% with oxidative cleavage products selectivity maintaining above 63.1%, suggesting excellent reusability of the WO3–STS catalyst. In addition, the tungsten leaching of the WO3–STS catalyst is controlled below 2% for each reaction cycle (Fig. 4c), and it exhibits excellent mass stability. Due to the ignorable loss of WO3, the WO3–STS binary catalyst can maintain excellent performance during recycling reactions.
Further, in order to study the stability of WO3–STS catalyst, we analyzed the phase structure, morphology and micro region composition of the binary catalyst after it was recovered from the eighth reaction cycle by using XRD, STEM and EDS. The sample is denoted as WO3–STS-8. After the eighth recycle, the recovered catalyst remained most of its original diffraction peaks as fresh WO3–STS (Fig. 1). But the peak intensity decreases significantly especially for the peaks with diffraction angle lower than 10° which might be caused by decrease of crystal size. Nonetheless, the characteristic diffraction peaks at 2θ = 23.07°, 23.54°, 24.35°, 33.18° and 34.19° which are attributed to monoclinic WO3 crystal are discernible. Although it's hard to distinguish STS from WO3 since the characteristic peaks of STS overlap with WO3, it is safe to conclude that WO3 still exists as crystal. The nitrogen adsorption–desorption isotherms and pore size distribution were obtained for fresh WO3–STS and the one used for 8 cycles are provided in the ESI Fig. S1.† As can be seen from the results, the isotherms and pore size distribution remain nearly unchanged. The texture properties (Table S2†) reveals that after 8 recycles, specific area of micropores and pore volume decreased slightly.
Two different morphologies are observed in the TEM image, and three areas are marked according to the TEM image contrast (Fig. 5a). The elemental mapping results reveal that O, Si and Ti atoms distribute in area 1, 2 and 3, but W mainly appears in area 1 (Table 3). The elemental distribution was further analyzed by EDS (Fig. 5b–e). It confirms that W mainly located at area 1, and Si and Ti mainly located at area 3. For area 2, all Si, Ti and W atoms are discovered since two kinds of particles is mixed. The above analysis suggests that the particles in area 1 are mainly WO3, while the particles in area 3 are mainly STS zeolite. The intracrystalline mesopores in area 3 also proves its zeolite nature. Then, we employ HADDF characterization method to analyze the STS zeolite. It is surprise to find out that many sub-nano WO3 particles dispersed on the STS surface with diameter of 1–3 nm (Fig. 5f–h). These particles might be generated during the MO oxidative reaction. Since the morphology of WO3 in area 1 remains well, it is inferred that only part of WO3 involved the reaction and finally deposited on the surface of STS. This result also explains why W is discovered in area 3.
Fig. 6 MO conversion and products distribution along with reaction time for the WO3-catalyzed MO oxidative cleavage reaction. |
In order to figure out how the reaction occurred, we further carried out the WO3 catalyzed experiments with epoxide MES and diol MDS as starting materials, and the results are displayed in Table 4. It can be seen that MES is quite active in this reaction, 90% of it converts into NA, MAA and MDS with selectivity 36.0%, 35.5% and 28.5%, respectively. That is to say, oxidative cleavage and hydrolysis are both possible reactions for MES but the latter is more preferred. If all MDS is generated from MES in MO oxidative cleavage reaction, then MDS selectivity doesn't match the selectivity of NA and MAA in Fig. 6. Because according to Table 4, the selectivity of MDS in Fig. 6 should lower than that of NA or MAA if it is generated from MES. Therefore, most of MDS might be generated directly from MO. As for catalytic reaction of MDS, the result shows that is too stable to occur further reaction under the oxidative reaction condition.
Starting material | Conversion (%) | Selectivity (%) | |||||
---|---|---|---|---|---|---|---|
NA | PA | MAA | MHA | MES | MDS | ||
a n(starting material):n(H2O2):n(t-BuOH) = 1:2.5:20, m(WO3):m(starting material) = 0.15:10, temperature 80 °C, reaction time 4 h. | |||||||
MO | 91.7 | 14.2 | 1.1 | 13.1 | 0.9 | 20.2 | 50.5 |
MES | 90.0 | 36.0 | 0 | 35.5 | 0 | 0 | 28.5 |
MDS | 0 | 0 | 0 | 0 | 0 | 0 | 0 |
Based on the above results and analysis of WO3 catalyzed reactions, we speculated the possible reaction pathway of MO oxidation cleavage as depicted in Scheme 1. MO is firstly converted into epoxide (MES) and diol (MDS) products. MDS is relatively inert and cannot go further conversion under the reaction conditions. While MES is reactive and further undergoes hydrolysis to form MDS or oxidative cleavage to form NA and MAA. The aldehydes can be further oxidized to carboxylic acid. As the oxidative cleavage is stoichiometric reaction, the molar ratio of NA to MAA is close to 1:1. As mentioned above, STS is capable of catalyze the oxidation of MO to generate MES, so there would be more MES that could be converted to NA and MAA by WO3. And that's why the selectivity of NA and MAA is improved and to the opposite, the MDS selectivity is decreased (Table 2, entry 6).
The catalytic nature of STS doesn't explain for the improvement of reusability for WO3–STS in the recycling reaction. The deposition of WO3 on STS might matters. As previously discussed, the catalysis of WO3 on oxidative cleavage of MO is ensured, but how does this happen?. Through the interaction of WO3 with H2O2, peroxotungstate which is the key active species is generated. So MO could be epoxidated and further cleaved into targeted products through the interaction with it. And the peroxotungstate species would turn into polytungstate. Though insoluble in water, it could still react with H2O2 and forming the reactive peroxotungstate species and proceeding the MO oxidative cleavage reaction. If H2O2 is not depleted completely after the reaction, polytungstate would kept dissolving and generating peroxotungstate species which would lead to the loss of tungsten after separation of catalyst from liquid and thus lower down the reusability of the catalyst.
If H2O2 is decomposed and consumed, whether it can stop the formation of peroxotungstate species and retain tungsten in solid phase or not?. To verify this, we chose three types of tungsten containing compounds and reacted with H2O2 under the reaction condition except MO is absent from it. After the reaction, MnO2/Al2O3(10 w% MnO2) which was applied for peroxide compounds decomposition in the reaction mixture was added in and we waited until bubbles is not generating obviously. The tungsten concentration in the solution is measured by ICP-OES before and after adding MnO2/Al2O3 and the results are shown in Table 5. It clearly shows that though different in solubility due to the different tungsten containing compound, the concentration of homogeneous tungsten species decreases to lower than 1 mg kg−1. And that is to say, control the content of peroxide compounds in the liquid phase is the key to reduce the loss of tungsten.
Tungsten containing compounds | Tungsten concentration (mg kg−1) | |
---|---|---|
Before adding MnO2/Al2O3 | After adding MnO2/Al2O3 | |
a n(Tungsten containing compound):n(H2O2):n(t-BuOH) = 1:2.5:20, temperature 80 °C. | ||
WO3 | 138 | <1 |
H28N6O41W12 | 384 | <1 |
(NH4)10W12O41∼xH2O | 172 | <1 |
The H2O2 conversion along with reaction time during the MO oxidative cleavage reaction under different catalyst condition was analyzed by titration method and the results are depicted in Fig. 7. When no catalyst is employed, the H2O2 conversion is lower than 5%. The H2O2 conversion increases linearly with reaction time, and reaches to 43% after reaction for 4 h. Compared with WO3, STS is far more effective for catalyzing H2O2 conversion. Since MO conversion is restively low as catalyzed by STS (Table 2, entry 3), part of H2O2 in this experiment might be decomposed inefficiently. And this result confirms the peroxide decomposing effect for STS. As WO3–STS is used, an improved H2O2 conversion compared with STS is obtained. As can be seen from the above results, STS functions as epoxidation catalyst as well as peroxide decomposing catalyst.
Fig. 7 H2O2 conversion along with reaction time catalyzed by different catalyst. n(MO):n(H2O2):n(t-BuOH) = 1:2.5:20, m(WO3–STS):m(MO) = 1:10, temperature 80 °C. |
Cold-spray ionization(CSI) mass spectrometer (MS) was further used to analyze the distribution of peroxotungstate species. Four liquid samples of filtrate obtained from the product of Fig. 8b–e were analyzed by CSI-MS. Only two samples from Fig. 8b and d showed peroxotungstate signals as shown in Fig. 9. The signals were attributed to various homogeneous tungsten species, such us [HWO4]−(m/z = 249.08), [HWO3(O2)]− (m/z = 264.88), [H19WO10(O2)3]− (m/z = 458.89), [H20WO11(O2)3]−(m/z = 476.72), H17W2O10(O2)5]− (m/z = 705.43), H13W3O9(O2)6]− (m/z = 933.20). When STS was added to the filtrate (Fig. 8d), it was found that the tungsten species with high mass charge ratio disappeared (Fig. 8c). This results indicate that these tungsten species is not stable with the existence of STS, and that explain how the STS promoted the depletion of peroxides.
Fig. 9 CSI-MS (negative-ion mode) analysis results of the filtrate: (a) sample obtained from Fig. 8b, (b) sample obtained from Fig. 8d, (c) sample obtained from Fig. 8c, (d) sample obtained from Fig. 8e. |
The reaction mechanism of WO3-STS catalyzed MO oxidative cleavage is proposed and depicted in Scheme 2. The oxidative cleavage reaction of MO is a two-step process and the epoxide MES is the key intermediate for the whole conversion. To increase the yield of oxidative cleavage products (NA and MAA), it is necessary to enhance the conversion of MO to MES. Both STS and WO3 are capable of active H2O2 and catalyze the expoxidation of MO. In this regard, adding STS into the reaction system would be a good choice due to their excellent catalytic activity for epoxidation.34,35 The epoxidation reaction catalyzed by both STS and WO3 supplies sufficient MES for the oxidative reaction. And the selectivity of unwanted diol product MDS which mainly formed directly from MO decreased obviously (Table 2, entry 4 and 6). Furthermore, WO3 is effective in converting MES into NA and MAA and it is the main catalyst to catalyze the MES oxidative cleavage reaction. Thus the binary WO3–STS catalyst shows high catalytic performance.
Due to the excessive H2O2, insoluble WO3 kept dissolving and forming soluble peroxotungstate and thus leading to the tungsten leaching. STS is capable of decomposing peroxide, therefore, the WO3 dissolving process is limited and insoluble tungsten species start to precipitate. When H2O2 was completely consumed, the tungstate decomposes into WO3 particles, which has poorer solubility, and these particles started to aggregate and precipitate. Because of the relatively large specific surface area of STS, it easy to efficiently capture these sub-nano WO3 particles and recover it. These WO3 particles are soluble to H2O2 and owing to the small size of it, it is easier to be peroxidized than bulk WO3 particles and the MO conversion is thus improved in the recycling reactions. Owing to the cooperation of STS and WO3, both good catalytic performance and reusability are achieved.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/d1ra08501h |
This journal is © The Royal Society of Chemistry 2022 |