DOI:
10.1039/D2RA05154K
(Paper)
RSC Adv., 2022,
12, 35959-35965
Co3O4@chitosan/La2O3 nanocomposites as innovative, powerful, and recyclable nanocatalysts for sonochemical treatment of benzyl alcohols to obtain the corresponding benzaldehyde derivatives†
Received
17th August 2022
, Accepted 1st October 2022
First published on 15th December 2022
Abstract
Ultrasonic (US) irradiation (100 W, 40 kHz) reactions, used as a safe and green technique, are often more efficient than traditional protocols. This leads us to introduce, for the first time, an efficient nanocatalyst and immobilization of La2O3 nanoparticles on Co3O4 nanoparticles for the selective oxidation of benzyl alcohol to the corresponding benzaldehyde at room temperature. The structural and morphological characteristics of the nanocatalysts were determined by FT-IR, XRD, FE-SEM, EDX, and VSM. The catalytic performance of the Co3O4@Cs/La2O3 composites used as heterogeneous nanocatalysts was investigated in the selective oxidation of benzylic alcohols to their corresponding benzaldehydes. Also, the performance of the oxidation parameters, including H2O2 concentration, time, effect of various solvents, and nanocatalyst dosage was checked. Significant benefits of this method can be named by using a non-toxic solvent, easy product isolation, excellent recoverability, low time of reaction, high yield, and ultrasound irradiation. Finally, a possible mechanism was proposed to show the nanocatalytic process.
1. Introduction
One of the most challenging functional group transformations for good chemical production in both the laboratory and at industrial scale is considered to be the selective oxidation of benzyl alcohol to its corresponding benzaldehyde (BZD).1,2 Generally, conventional inorganic and traditional oxidants such as Cr(VI) oxides, pyridinium chlorochromate (PCC), and permanganate (MnO4−), and so on, are toxic, unstable, expensive, and hazardous to use.2 Therefore, they produce a great amount of toxic waste, the recovery of which requires many extra chemical processes that are expensive and dangerous. Thus, it is not economically feasible and causes environmental danger. Therefore, from the perspective of green chemistry and being ecofriendly, the use of such oxidation should be avoided. Recently, environmental pollution has become one of the most important challenges, and for this reason, chemists are choosing reactants, the reaction products of which cause the lowest pollution and hazards to the environment. So, hydrogen peroxide (H2O2) is a strong, green, cheap, mild, and ecofriendly oxidizer, and its only by-product is H2O. Thanks to its special and attractive properties, chemists have assigned a great amount of time to researching the uses of H2O2.6,7
In terms of quantity used, BZD (with a smell of bitter almonds) is the second most important aromatic molecule (after vanillin). In this field, the catalytic processes that lead to excellent-quality BZD are particularly appealing for use in the perfume and food industries, pharmaceuticals, dyes, beverages, agribusiness industries, and chemicals.3–7
The most plentiful polysaccharide, other than cellulose, is chitin, which has many properties such as biodegradability and biocompatibility.8 Chitosan (CS) is the basic derivative of chitin. Recently, CS has attracted the attention of chemists due to its abundant properties such as inexpensiveness, it is an abundant resource, hydrophilicity, environmentally friendliness, nontoxicity, excellent chemical and thermal stability, and its antifungal, antibacterial, and antioxidant properties. Also, the NH2 and OH groups in the CS structure provide diverse coordination sites for chemical modifications such as chelating ligands to coordinate different metal ions to synthesize magnetic composites,7–12 (Scheme 1).
|
| Scheme 1 Chitosan structure. | |
Recently, cobalt oxide (Co3O4) nanoparticles (NPs) have become an important, magnetic, and well-known p-type semiconductor that has increasingly attracted attention because it is inexpensive and ecofriendly, is simple to prepare and has high chemical and physical stability. The Co3O4 has been studied because it is a promising substance with a great number of applications in lithium-ion batteries, gas sensing, information storage, heterogeneous catalysis, optical devices, magnetic materials, and electrochromic devices.13–15 Co3O4 with valence of more than 3 is unstable in the normal environment. However, other cobalt oxide forms such as Co3O4 and CoO, are more stable and have more advantages in industrial applications.16
Lanthanum oxide (La2O3) one of the rare earth oxides, has been investigated as a catalyst in different reactions because of its unique properties (excellent paramagnetic sensitivity, saturated magnetism, constriction magnetic properties, large bandgap, and so on). It is also a good candidate for studies because of its significant applications in electronics, sensors, insulators, antimicrobial agents, biomedicine, and biocatalysts. Therefore, La2O3 is an excellent choice for research on improving its catalytic activity.1,2,6,7,17–19
In addition, the ultrasound (US) irradiation method is an ecofriendly, safe, and cheap technology which is used as a versatile tool in a vast range of scientific and technological applications.20–22 In contrast to normal thermal heating, US irradiation has many important benefits: improved efficiency, a significant reduction in reaction time, increased selectivity, it is inexpensive and easy to handle and use in various procedures, and the compounds show excellent purity. Additionally, in many cases, reactions under US irradiation could be considered as being ecofriendly procedures and use a small number of solvents.23,24 Therefore, US irradiation causes the least number of side reactions.25
In this regard, a fast and green method for the synthesis of Co3O4@Cs/La2O3 nanocomposites for use as novel heterogeneous nanocatalysts is proposed and its efficiency in the oxidation of benzyl alcohol to BZD is also explored. We developed the oxidation of benzyl alcohol to BZD at room temperature and under US conditions. As understood from this proposed procedure, it greatly complements the goals of green chemistry, and it can be used effectively in the production of BZD, with the use of the Co3O4@Cs/La2O3 nanocomposites as a nanocatalyst. It also shows massive advantages for both use in industry and academia.
2. Results and discussion
The Fourier transform infrared (FT-IR) spectrum of Co3O4@Cs/La2O3, Co3O4, and pure CS are shown in Fig. 1. The two strong absorbance bands at about 561 and 660 cm−1 (565 and 661 cm−1) were ascribed to the Co–O stretching vibrations (Fig. 1a and c).16,26 The absorption bands at 3364, and 3434 cm−1 were ascribed to the amino and hydroxyl groups of CS, and also the bands at 1384 and 1374 cm−1 were related to the C–O stretching vibration of the hydroxyl groups of CS. The bands at 1649 and 1635 cm−1 corresponded to the CO stretching vibration of the amide group (Fig. 1b and c).27–30 The characteristic bands at 419 cm−1 were due to the La–O stretching band (Fig. 1c).6,7,31
|
| Fig. 1 The FT-IR spectra of (a) Co3O4, (b) pure CS, and (c) Co3O4@Cs/La2O3 nanocomposites. | |
In the energy-dispersive X-ray spectroscopy (EDX) spectrum shown in Fig. 2, the presence of the elements: C, Co, La, N, and O, was determined according to their energy, which indicated the confirmation of the product purity.
|
| Fig. 2 The EDX spectrum of Co3O4@Cs/La2O3. | |
Data obtained from the X-ray diffraction (XRD) analysis, which was used in analysis of the Co3O4@Cs/La2O3 catalyst synthesized in this project, is shown in Fig. 3. The XRD samples for Co3O4, CS, La2O3 NPs, and the Co3O4@Cs/La2O3 nanocomposite are shown in Fig. 3a–d. The developed peaks indicate the dimensions of the nano sized particles. The characteristic peaks for Co3O4 are found in the region at 2θ of 31.3°, 36.89°, 44.83°, 55.61°, 59.43°, and 65.42°, which corresponded to (220), (311), (400), (422), (511), and (440), respectively. The network parameters agreed well with those of the JCPDS card number 01-078-1969 (standard cubic Co3O4).32 The broad diffraction peaks of CS show 2θ = 10.60 and 19.9° and it was a good match with the results given in past reports.6,33 Also, the La2O3 NPs had peaks that are shown at 27.2912°, 28.3643°, 39.6213°, and 46.4585° and are related to La2O3, which correspond to (222), (300), (400), and (622), respectively, (La2O3, JCPDS card no. 04-0856).34 Characteristic peaks for Co3O4 and La2O3 indicated that the structure of them both had not changed during the combination process.
|
| Fig. 3 The XRD patterns of (a) Co3O4, (b) CS, and (c) La2O3 and Co3O4@Cs/La2O3. | |
Scanning electron microscopy (SEM) is a powerful technique for investigating surface morphology. The morphology, size, and form of the catalyst were surveyed by SEM at different magnifications. The result was that the FE-SEM images showed a magnetic Co3O4@Cs/La2O3 nanocomposite consisting of nearly spherical particles with a size of about 32–35 nm (Fig. 4).
|
| Fig. 4 The FE-SEM images, at different magnifications, of the Co3O4@Cs/La2O3 catalyst, (a) 1 μm, (b) 200 μm, and (c) 2000 nm. | |
The magnetic behaviors of Co3O4 and Co3O4@Cs/La2O3 were determined using a vibrating sample magnetometer (VSM) at room temperature (Fig. 5). There was no hysteresis, coercivity, or remanence in bare Co3O4 and Co3O4@Cs/La2O3 samples at room temperature, which showed their typical superparamagnetic behavior. The Co3O4 NPs and Co3O4@Cs/La2O3 had superparamagnetic behavior, which facilitated the magnetic separation. The saturation magnetization values (Ms) of the Co3O4NPs and Co3O4@Cs/La2O3 nanocomposites were 46.5 and 25.8 emu g−1, respectively. However, the addition of the CS layer and the La2O3 NPs on the Co3O4 surface results decreased the magnetic behavior, and the Co3O4@Cs/La2O3 nanocomposite saturation magnetization was sufficient for a rapid magnetic separation by an external magnet.7,35
|
| Fig. 5 The VSM results, (a) Co3O4, and (b) Co3O4@Cs/La2O3 nanocomposites. | |
2.1. Catalytic activity of Co3O4@Cs/La2O3 nanocomposites
The catalytic activity of the Co3O4@Cs/La2O3 was compared with that of various catalysts to determine the requirement for the presence of a catalyst for the oxidation of benzyl alcohols (Table 1). The oxidation of benzyl alcohols to the corresponding BZDs was performed under a mild reaction and sonochemical conditions. Oxidation under sonication conditions plays a fundamental role in this process. Also, the benzyl alcohols were oxidized both in the presence of, and without the Co3O4@Cs/La2O3 nanocatalyst (Table 1, entries 5–8). The yield of BZD obtained was established to be only 58%, 63%, 80%, 85%, and 97% in the presence of 50 mg of Co3O4@Cs/La2O3 and different solvents (Table 1, entries 1–5), respectively. The oxidation of benzyl alcohol was carried out using 50 mg of Co3O4@Cs/La2O3 without any solvent. Also, the yield of BZD formation without a catalyst was decreased (Table 1, entry 8). When the catalyst amount was increased, the BZD was obtained with a lower yield (Table 1, entry 9). In Table 1, a large comparison of the catalytic activities of Co3O4@Cs/La2O3 with other catalysts used in the oxidation of benzyl alcohol is shown (Table 1, entries 12–20). It was concluded, that the catalyst gave excellent results and offered very gentle reactions conditions and was a green option.
Table 1 The effect of different conditions on the benzyl alcohol oxidationa
Table 2 summarizes the results from the Co3O4@Cs/La2O3 nanocatalyst oxidation reactions. A wide range of aromatic alcohols has been change to benzaldehyde derivatives with great yields within a short reaction time at room temperature (Table 2). Both electron-donating and electron-withdrawing groups accelerated the oxidation reaction, but the presence of any steric hindrance around the hydroxyl group of the benzyl alcohol substituent at the ortho or meta position caused decreased yields and a longer reaction time (Table 2, entries 1, 4, 6, 8, 9 and 11). However, when compared with the para position, because of the absence of steric hindrance, there was an increase in the yield and a decrease in time.6,36,37
Table 2 Oxidation of benzyl alcohols to benzyl aldehydesa
|
Entry |
X |
Time (min) |
Yieldb (%) |
Selectivity (%) |
Reaction conditions: benzyl alcohols (1 mmol), H2O2 (1 ml), Co3O4@CS/La2O3 (0.05 g). Isolated yield. |
1 |
3-Hydroxy |
10 |
87 |
>99 |
2 |
4-Hydroxy |
8 |
97 |
>99 |
3 |
4-Chloro |
8 |
97 |
>99 |
4 |
2-Chloro |
10 |
83 |
>99 |
5 |
4-Methoxy |
8 |
96 |
>99 |
6 |
3-Methoxy |
10 |
90 |
>99 |
7 |
4-Methyl |
8 |
97 |
>99 |
8 |
3-Methyl |
10 |
92 |
>99 |
9 |
3-iPr |
12 |
87 |
>99 |
10 |
4-Nitro |
8 |
96 |
>99 |
11 |
3-Nitro |
10 |
87 |
>99 |
12 |
4-Fluoro |
8 |
95 |
>99 |
13 |
4-Bromo |
8 |
96 |
>99 |
14 |
3-Bromo |
10 |
83 |
>99 |
15 |
Benzyl alcohol |
8 |
97 |
>99 |
According to all this information and the investigation, an acceptable mechanism for this oxidation was proposed. The results demonstrated that La3+ (on the surface of Co3O4@Cs/La2O3) acts as a Lewis acid site in the oxidation of benzyl alcohols. The La3+ was coordinated to the oxygen of the peroxide hydrogen and formed an La–OOH intermediate A as the first step. In the second step, intermediate A reacted with benzyl alcohols to form intermediate B, and the deletion of an H2O molecule from intermediate B, resulted in intermediate C, and at the end, it resulted in the elimination of the secondary H2O molecule and created the corresponding BZD (Scheme 2).6,36–38
|
| Scheme 2 A possible reaction mechanism. | |
2.2. Catalyst reutilization
For catalytic activity, stability plays an essential role. In this project, the catalyst reusability of the Co3O4@Cs/La2O3 was investigated under optimum reaction conditions. The results showed that the Co3O4@Cs/La2O3 was recovered up to the fifth cycle (Fig. 6). The results of the XRD analysis of the Co3O4@Cs/La2O3 nanocatalysts after five cycles of reuse are shown in Fig. 7b. The characteristic peaks for Co3O4@Cs/La2O3 were conserved, showing that the nanocatalysts had been very stable and pure.
|
| Fig. 6 Recyclability of the sonocatalyst. | |
|
| Fig. 7 Comparison of the XRD spectra of the prepared Co3O4@Cs/La2O3 (a) before, and (b) after five runs. | |
3. Experimental
3.1. Chemicals and apparatus
For this work, all the high quality material and chemicals, including alcohol and solvents needed for the experiments, were purchased from Merck and the Aldrich Company. The FT-IR spectroscopy samples were dispersed in KBr and then made into pellets and their spectra were acquired using a PerkinElmer 1600 FTIR spectrometer. In addition, the morphology and size of the samples were determined by SEM, and the crystals were investigated by XRD, EDX, and VSM. The oxidation yields were investigated using gas chromatographic spectrometry (GC).
3.2. Preparation of the Co3O4 nanoparticles
The Co3O4 NPs were fabricated according to method found in the literature and were obtained successfully. Approximately 8.60 g of cobalt(II) nitrate was dissolved in 100 ml of EtOH for about 30 s, in a round bottomed flask. Then, 2.14 g of ethanedioic acid was slowly added and the reaction mixture was stirred for 2 h at 45 °C. The precipitate formed consisted of cobalt(II) oxalate powder and was collected by centrifugation followed by calcining at 400 °C for 2 h to produce the Co3O4 NPs.45
3.3. Preparation of Co3O4@CS
The Co3O4@Cs nanocomposites were synthesized according to our previous method.7 The Co3O4@CS nanocomposites were prepared by dispersing 0.01 g CS dissolved in 10 ml of ethanoic acid. Next, 0.25 g of Co3O4 was added to the CS solution and dispersed for 30 min. The reaction mixture was mechanically stirred at 60 °C. Subsequently, a solution was made by dissolving 0.02 g of sodium tripolyphosphate (STPP) in 50 ml of deionized water, which was added dropwise at a rate of 4.5 ml h−1. At this step, the ionic gelation of CS occurred on the Co3O4 MNP surface. Next, after filtration, the reaction mixture was dried for 36 h at −20 °C. Finally, the core–shell product of the Co3O4@Cs NPs was obtained.
3.4. Procedure for the preparation of Co3O4@Cs/La2O3
The Co3O4@Cs/La2O3 nanocomposites were prepared according to our previous method.6,7 The Co3O4@Cs/La2O3 nanocomposites were created by dispersing about 0.1 g of Co3O4@Cs in deionized water (50 ml) and sonicating the mixture for 60 min. Subsequently, 0.05 g of LaCl3·7H2O was added. The reaction mixture was stirred for about 120 min under reflux conditions. Finally, the products were separated by centrifugation, and then washed three times with distilled water.
3.5. General procedure for the oxidation of benzyl alcohols
A mixture of benzyl alcohol (1 mmol), H2O2 (1 ml) and Co3O4@Cs/La2O3 (0.05 g) was added to a round bottomed flask and the mixture was sonicated in an ultrasonic bath (constant frequency) at 25 °C. After the completion of the oxidation, as determined out by thin-layer chromatography (TLC), the magnetic catalyst was separated using an external magnet.7
4. Conclusions
In conclusion, we designed and investigated Co3O4@Cs/La2O3 nanocatalysts. Also, the oxidation of benzyl alcohol derivatives to different benzaldehydes using the Co3O4@Cs/La2O3 nanocatalysts was carried out at room temperature under ultrasonic irradiation conditions. Using the previously mentioned conditions, the catalytic activity of nanocatalysts for the selective oxidation of benzyl alcohols to benzaldehyde was investigated (Table 2). The benzyl alcohol derivatives were oxidized to the corresponding benzaldehyde, with excellent yield, within 8 min. Benzaldehydes are known to be significant intermediates, which are oxidized by benzyl alcohol in industry and chemistry. Therefore, the mechanism of the oxidation of benzyl alcohol is of particular importance for organic chemists. Some of the properties of the Co3O4@Cs/La2O3 nanocatalysts include a decreased reaction time, the ability to be easily separated magnetically, the retention of excellent chemical stability after five periods of reuse, increased selectivity, and high yield.
Conflicts of interest
The authors state that they had no financial or personal conflicts of interest in preparing the materials reported in this article.
References
- J. Yang, K. Cao, M. Gong, B. Shan and R. Chen, J. Catal., 2020, 386, 60–69 CrossRef CAS.
- T. Tamiji and A. Nezamzadeh-Ejhieh, Mater. Chem. Phys., 2019, 12, 121813 CrossRef.
- R. Hudson, Y. Feng, R. S. Varma and A. Moores, Green Chem., 2014, 16, 4493–4505 RSC.
- J. C. Colmenares, W. Ouyang, M. Ojeda, E. Kuna, O. Chernyayeva, D. Lisovytskiy, S. De, R. Luque and A. M. Balu, Appl. Catal., B, 2015, 183, 107–112 CrossRef.
- M. J. Jacinto, P. K. Kiyohara, S. H. Masunaga, R. F. Jardim and L. M. Rossi, Appl. Catal., A, 2008, 338, 52–57 CrossRef CAS.
- F. Javidfar, M. Fadaeian and J. Safaie Ghomi, Polycyclic Aromat. Compd., 2021, 1–11 Search PubMed.
- F. Javidfar, M. Fadaeian and J. Safaei Ghomi, RSC Adv., 2021, 11, 35988–35993 RSC.
- M. Nasrollahzadeh, N. Shafiei, Z. Nezafat, N. Sadat Soheili Bidgoli and F. Soleimani, Carbohydr. Polym., 2020, 241, 116253 CrossRef.
- J. Safari, F. Azizi and M. Sadeghi, New J. Chem., 2015, 39, 1905–1909 RSC.
- J. Safari and Z. Zarnegar, RSC Adv., 2014, 4, 20932–20939 RSC.
- Y. Xie, X. Liu and Q. Chen, Carbohydr. Polym., 2007, 69, 142–147 CrossRef CAS.
- D. H. K. Reddy and S. M. Lee, Adv. Colloid Interface Sci., 2013, 68, 201–202 Search PubMed.
- A. B. Vennela, D. Mangalaraj, N. Muthukumarasamy, S. Agilan and K. V. Hemalatha, Int. J. Electrochem. Sci., 2019, 14, 3535–3552 CrossRef CAS.
- T. O. Ahmadova, Z. Durmusa, A. Baykala and H. Kavasb, Inorg. Mater., 2011, 47, 426–430 CrossRef.
- C. Ramamoorthy and V. Rajendran, Optik, 2017, 145, 330–335 CrossRef CAS.
- S. A. Makhlouf, et al., Superlattices Microstruct., 2013, 64, 107–177 CrossRef CAS.
- H. Dabhane, S. Ghotekar, P. Tambade and V. Medhane, Asian. J. Nano. Mat., 2020, 3, 291–299 CAS.
- X. Long, L. He, W. Ye and Q. Sun, J. Electron. Mater., 2020, 49, 6611–6621 CrossRef CAS.
- C. Jin, Q. Yao, J. Li, B. Fan and Q. Sun, Mater. Des., 2015, 15, 205–210 CrossRef.
- J. A. Fuentes-García, J. Santoyo-Salzar, E. Rangel-Cortes, G. F. Goya, V. Cardozo-Mata and J. A. Pescador-Rojas, Ultrason. Sonochem., 2020, 105274 Search PubMed.
- J. Wang, J. Fan, J. Li, X. Wu and G. Zhang, Ultrason. Sonochem., 2018, 48, 404–411 CrossRef CAS PubMed.
- E. A. Dil, M. Ghaedi, A. Asfaram, F. Zare, F. Mehrabi and F. Sadeghfar, Ultrason. Sonochem., 2017, 39, 374–383 CrossRef PubMed.
- G. Zbancioc, O. Florea, P. Jones and I. I. Mangalagiu, Ultrason. Sonochem., 2012, 19, 399–403 CrossRef CAS PubMed.
- M. Nikpassand, L. Z. Fekri and P. Farokhian, Ultrason. Sonochem., 2016, 28, 341–345 CrossRef CAS PubMed.
- J. P. Hallett and T. Welton, Chem. Rev., 2011, 111, 3508–3576 CrossRef CAS.
- M. Salavati-Niasari and A. Khansari, C. R. Chim., 2014, 17, 352–358 CrossRef CAS.
- J. Safari and L. Javadian, RSC Adv., 2014, 4, 48973–48979 RSC.
- J. Safari and L. Javadian, Ultrason. Sonochem., 2015, 22, 341–348 CrossRef CAS PubMed.
- J. Safari, F. Azizi and M. Sadeghi, New J. Chem., 2015, 39, 1905–1909 RSC.
- J. Safari and Z. Zarnegar, RSC Adv., 2014, 4, 20932–20939 RSC.
- N. Sulaiman, Y. Yulizar and D. O. B. Apriandanu, AIP Conf. Proc., 2017, 020105 Search PubMed.
- U. Aftab, A. Tahira, A. Gradone, V. Morandi, M. I. Abro, M. M. Baloch and Z. H. Ibupoto, Int. J. Hydrogen Energy, 2021, 46, 9110–9122 CrossRef CAS.
- M. Jiang, et al., Int. J. Biol. Macromol., 2010, 47, 696–699 CrossRef CAS PubMed.
- P. Hou, C. Shi, L. Wu and X. Hou, Microchem. J., 2016, 128, 218–225 CrossRef CAS.
- A. A. Pathan, K. R. Desai and C. P. Bhasin, Int. J. Nano. Chem., 2017, 3, 21–25 CrossRef.
- A. R. Hajipour, H. Karimi and A. Koohi, Chin. J. Catal., 2015, 36(7), 1109–1116 CrossRef CAS.
- A. R. Hajipour and H. Karimi, Chin. J. Catal., 2014, 35(9), 1529–1533 CrossRef CAS.
- L. Laasri, M. El Makhfi and S. Sebti, Mater. Today., 2020, 31, S156–S161 CAS.
- S. Tareq, Y. H. T. Yap, T. A. Saleh, A. H. Abdul Halim Abdullah, U. Rashid and S. M. Izham, J. Mol. Liq., 2018, 271, 885–891 CrossRef CAS.
- P. Wang, J. Cai, J. Yang, C. Sun, L. Li, H. Hu and M. Ji, Tetrahedron Lett., 2013, 54, 533–535 CrossRef CAS.
- S. Rautiainen, O. Simakova, H. Guo, A.-R. Leino, K. Kordás, D. Murzin and D. T. Repo, Appl. Catal., A, 2014, 485, 202–206 CrossRef CAS.
- H. Su and C. Yang, Chin. J. Catal., 2014, 35, 1224–1234 CrossRef CAS.
- S. Farhadi, Z. Babazadeh and M. Maleki, Acta Chim. Slov., 2006, 53, 72–76 CAS.
- B. Karimi, F. B. Rostami, M. Khorasani, D. Elhamifar and H. Vali, Tetrahedron, 2014, 70, 6114–6119 CrossRef CAS.
- C. C. Lin, Y. Guo and J. Vela, ACS Catal., 2015, 5, 51037–51044 Search PubMed.
|
This journal is © The Royal Society of Chemistry 2022 |
Click here to see how this site uses Cookies. View our privacy policy here.