Matteo Andrea
Lucherelli†
,
Víctor
Oestreicher†
,
Marta
Alcaraz
and
Gonzalo
Abellán
*
Instituto de Ciencia Molecular (ICMol), Universidad de Valencia, Catedrático José Beltrán, 46980, Paterna, Valencia, Spain. E-mail: gonzalo.abellan@uv.es
First published on 21st April 2023
The layered allotropes of group 15 (P, As, Sb and Bi), also called two-dimensional (2D) pnictogens, have emerged as one of the most promising families of post-graphene 2D-materials. This is mainly due to the great variety of properties they exhibit, including layer-dependent bandgap, high charge-carrier mobility and current on/off ratios, strong spin–orbit coupling, wide allotropic diversity and pronounced chemical reactivity. These are key ingredients for exciting applications in (opto)electronics, heterogeneous catalysis, nanomedicine or energy storage and conversion, to name a few. However, there are still many challenges to overcome in order to fully understand their properties and bring them to real applications. As a matter of fact, due to their strong interlayer interactions, the mechanical exfoliation (top-down) of heavy pnictogens (Sb & Bi) is unsatisfactory, requiring the development of new methodologies for the isolation of single layers and the scalable production of high-quality flakes. Moreover, due to their pronounced chemical reactivity, it is necessary to develop passivation strategies, thus preventing environmental degradation, as in the case of bP, or controlling surface oxidation, with the corresponding modification of the interfacial and electronic properties. In this Feature Article we will discuss, among others, the most important contributions carried out in our group, including new liquid phase exfoliation (LPE) processes, bottom-up colloidal approaches, the preparation of intercalation compounds, innovative non-covalent and covalent functionalization protocols or novel concepts for potential applications in catalysis, electronics, photonics, biomedicine or energy storage and conversion. The past years have seen the birth of the chemistry of pnictogens at the nanoscale, and this review intends to highlight the importance of the chemical approach in the successful development of routes to synthesise, passivate, modify, or process these materials, paving the way for their use in applications of great societal impact.
2D-Pn materials have witnessed increasing attention because their properties can meet the limitations of graphene, such as the absence of band-gap or the pronounced chemical inertness, features that, for example, have precluded the development of highly efficient electronic micro-devices. For this reason, semiconducting 2D black phosphorus (bP) has emerged as a promising alternative to fill this gap.2 Moreover, 2D-Pn exhibit a great variety of physical properties like tunable layer-dependent bandgap, ballistic transport, or strong spin–orbit coupling, to name a few, thus making these materials very promising for (opto)electronic applications, like solar cells or field effect transistors (FET) as well as for spintronic devices.9 Moreover, from a chemical point of view, 2D-Pn are also particularly appealing due to their monoelemental nature (which simplifies its study), their high specific- and volumetric-capacities when used as electrode materials for energy storage systems, or their excellent behaviour as heterogeneous catalysts.11 Altogether, 2D-Pn exhibits a wide range of physical and chemical properties that can be exploited in different applications of great social importance, however, several challenges related to its stability, processing or large-scale production must be overcome.
Before guiding the readers to the nanoscale properties of 2D-Pn, is it worth recalling their elemental bulk properties keeping in mind to better trace the current research development. Their first classification from the Periodic Table suggests a marked difference between them, with N and P belonging to non-metals elements, while As and Sb are considered metalloids and Bi a metal. These last three members are commonly known as heavy pnictogens. Elemental nitrogen is the only one that exists as a molecular gas under environmental conditions, N2. In the case of phosphorus, a wide variety of allotropes can be found, ranging from molecular to extended solids. Specifically, white phosphorus is an air-sensitive molecular solid composed of P4 entities.
Among the extended phases, while the red phosphorus is an amorphous polymeric solid, the violet, black and blue phosphorus are crystalline structures, being bP the most stable one. It is worth noting that black and blue phosphorus are layered structures, also known as α and β structures, respectively. Analogously, arsenic also can be found as a molecular solid (As4, more stable than white phosphorus), showing both α- and β-layered structures. Finally, antimony and bismuth elements are mainly found as extended crystalline solids, being the β form the most stable one.9
Concerning their layered structures, α-form exhibits an orthorhombic disposition where the atoms are arranged in a six-member rings pucked structure (Fig. 1A), while the β-form displays a rhombohedral structure (Fig. 1B). Indeed, bP's will be mainly found in its α-form, while the other Pn members exhibit the β-one. Additionally, the α and β structures affect the bulk nature of their allotropes, as in the case of the heavier 2D-Pn that are characterised by strong interlayer interactions (higher than in graphene) increasing from As to Bi, associated with the corresponding increment of their metallic character.9,12 This aspect is crucial for 2D-Pn production, which we will further discuss below.
Fig. 1 Schematic representation of α- and β-layered structures of Pn. (A) Top and side views of the orthorhombic structure (Cmce space group), corresponding to the most stable thermodynamic form of P as bP. (B) Top and side views of the rhombohedral structure (R3m space group), corresponding to the most stable thermodynamic form of As, Sb and Bi. The insets show aberration-corrected STEM atomic-resolution HAADF images (not corresponding with the orientation shown in the crystal structure sketches) measured at 80 kV of 2D-α-BP (Fourier filtered) and 2D-β-Sb, respectively.11,13 Characteristic distances and angles according to the crystal structure. |
From the chemical point of view, tabulated redox potentials give a straightforward idea of the chemical reactivity in terms of the redox reactions for bulk Pn, which can be easily visualised in a Frost diagram (for sake of clarity N has been avoided).14 As depicted in Fig. 2, and calculated under acidic aqueous conditions, negative oxidation states are available for all the Pn members. In the case of the oxidation state (−3), the reducing strength decreases from P to Bi in comparison with the zero valent species. In the case of the highest oxidation state (+5), all the Pn have positive reduction potential except P, showing its particularly high tendency towards oxidation. Since Frost diagrams are based on reduction potentials measured in aqueous solution, this can be considered as a first input pointing out the different stability of bP in comparison to the other Pn analogues. This results in the well-known oxophilic behaviour of phosphorus, which triggers the low environmental stability of bP.15 In the case of the other pnictogens, the oxidation tendency decreases from Bi to As, for both oxidation states: +3 or +5.
Fig. 2 Frost diagram for Pn elements under acidic aqueous conditions. Image reproduced with permission from ref. 14. |
Furthermore, in the 2D limit, due to the presence of the extra nonbonding electron pair in every single atom, the surface of these layered materials can be considered as a massive delocalized 5 electron cloud, endowing the materials with a characteristic chemical feature. For instance, in the case of bP, this behaviour could play the role of a soft nucleophile in certain types of chemical reactions.11 This provides a characteristic chemical reactivity to 2D-Pn that needs to be explored. Additionally, as soon as the principal quantum number increases, the radial distribution function of the p orbitals extends, thus the interlayer interaction becomes stronger, making their exfoliation complicated. This effect, which can be rationalised as a function of the out-of-plane:in-plane ratio, hinders the obtaining of few-layer flakes with large areas by top-down techniques, as generally demonstrated by Backes et al,6 and even proved by our group in the case of μME Sb flakes.16
Different is the case when the layered materials also present electrostatic interactions, such as layered double hydroxides. Here, the electrostatic energy is summed to the typical van der Waals interlayer interactions observed in 2D materials. Therefore, the delamination process required the stabilisation of charged layers as well as the solvation of intercalated anions.17–20 Along this article we will introduce the important double role played by the solvent in Pn's exfoliation process: physical (colloidal stability) and chemical (passivation, protective layer) stabilisation of the colloidal suspension.
With respect to the electronic properties of 2D-Pn, one of the most interesting points is their acute band gap layer-dependency. Indeed, bulk bP was reported to have a band gap of ∼0.31 eV, that increases with the reduction of the layer number, reaching ∼2 eV for monolayer bP.2 This increment in the band gap has been also calculated by DFT and reported for the other Pn, showing from metallic (trilayer As, bilayer Sb, and trilayer Bi) to insulator or semiconductor behaviour in the case of the monolayer (2.49, 2.28, and 0.32 eV for As, Sb and Bi, respectively).9,21,22
Regarding preparation methods, the more established approaches for other 2D systems such as graphene or TMDs have been successfully used for the production of bP and antimonene.23–25 Interestingly, the isolation of 2D bP has undergone a similar historical development as that of graphene. Indeed, despite its discovery dating to 1914,3 and its crystallographic description to 1935,4 its introduction in the realm of 2D material's family took almost 100 years. Indeed, the first isolation of single-layer bP (phosphorene) only occurred in 2014.2 Considering graphene as a reference example, bP can be produced by using common top-down techniques, including liquid phase exfoliation (LPE),24,26 electrochemical exfoliation,27–29 and bottom-up methods, such as CVD,30 pulsed laser deposition (PLD),31 and even solvothermal synthesis.32 Similarly, also for As, Sb and Bi bottom-up and top-down approaches have been developed, but in this case with disparate success.23,33–36 Indeed, the exfoliation of Pn using top-down routes like LPE is less efficient compared to other 2D materials. This is due to the external energy (e.g. sonication) required to overcome the strong interlayer interactions resulting in crystals breaking and downsizing (typically <300 nm in lateral dimensions), leading to non-homogeneous sheet morphologies.37 As the interlayer interactions increase along the group, highly anisotropic 2D-Bi flakes will be extremely difficult to achieve by LPE or related top-down approximations. Hence, the most promising route for the synthesis of heavy Pn lies in the use of bottom-up approaches.38,39 In fact, large-scale production of high-quality layered heavy Pn has been demonstrated by colloidal synthesis,40 a strategy that relies on chemists’ background.
In this feature article, we will present the research contribution carried out by our group and close collaborators on the emergent field of 2D-Pn nanomaterials emphasising the chemical approach as a promising alternative for the synthesis and investigation of their properties. To this aim, we are proposing and will employ along the manuscript a careful distinction of Pn's production. Specifically, the term “synthesis” will be only employed for bottom-up approaches, referring to those methods involving molecular precursors and chemical reactions.
The fil rouge across our work encompasses several aspects of fundamental research on Pn materials that can be resumed as follows: (i) production and chemical control, (ii) development of fundamental knowledge on the characterization, and (iii) research on the properties and applications of 2D-Pn. This article will guide the reader through 2D-Pn development, highlighting our contribution to its research and presenting our vision toward the future of these materials, discussing the key role that chemists should play in this exciting research field (Scheme 1).
Fig. 3 General scheme of the liquid phase exfoliation and sequential size selection through liquid cascade centrifugation (A). Photograph of a dispersion of exfoliated FL-bP in CHP (B). Low-resolution transmission electron microscopy (TEM) images of FL-bP exfoliated in CHP. Scale bar: 500 nm (C). Bright-field scanning transmission TEM (STEM) image of FL-bP. Scale bar: 2 nm (D). Butterworth-filtered high-angle annular dark field (HAADF) STEM image of FL-bP (exfoliated in isopropanol) showing the intact lattice. Scale bar: 1 nm (E). Histogram of the apparent thickness of the exfoliated FL-b1P obtained from AFM. Inset: Plot of the nanosheet length as a function of the flake height considering a total amount of 170 replicates. The average thickness is H = 11.5 ± 0.2 nm and lateral sizes are ranging from 45 to 475 nm (F). Sb flakes Raman A1g (λexc = 532 nm) mapping, where >14000 single point spectra over a surface area of 40 μm2 using a step size of 0.5 μm have been recorded (G). Plot of the nanosheet length as a function of the flake height (obtained from AFM), including the data corresponding to the control experiment for the ionic liquid, IL (H). Histogram of the apparent thickness of the exfoliated FL-Sb obtained from AFM (sample size = 271). The inset shows an AFM image of a nanosheet along with its corresponding height profiles of ca. 4 and 18 nm, respectively. Inset, scale bar: 100 nm (I). Figure adapted with permission from ref. 15 and 42. |
On the same pathway undertaken with bP, our group also contributed to the fundamental development of Sb-based 2D materials. Only a few months later after the first isolation of μME Sb monolayer by Zamora's group,43 we demonstrated the feasibility of the LPE approach for the 2D-Sb production. By applying tip sonication in i-propanol/water (4:1) mixture of grounded Sb crystals we were able to obtain few-layer Sb dispersions. Interestingly, in both cases, the material resulted to be stable for months under ambient conditions.42
Applying the knowledge developed for bP, we explored the correlation between thickness and number of layers by means of AFM and Raman spectroscopy. Our experimental observation showed a pronounced decrease of the Raman intensity with the number of layers, reaching silent spectra for the thinnest flakes, in contrast to other 2D materials like graphene or boron nitride. This decrease in the intensity was supported by DFT calculations, however, the complete disappearance of the Raman signal was related to the surface oxidation of the flakes as explained below.
For the preparation of unoxidized few-layers Sb, the ionic liquid (IL) 1-butyl-3-methylimidazolium tetrafluoroborate (bmim-BF4) was used on the basis of its excellent oxidation protection behaviour for FL-bP.11 Sonication of ground Sb crystals dispersed in bmim-BF4 was performed in an argon-filled glovebox (<0.1 ppm of H2O and O2) to yield brownish, open-air stable suspensions of unoxidized FL-Sb nanosheets, after removing the unexfoliated particles by a two-step centrifugation process. These samples exhibited median values of 310 nm in lateral dimensions and ca. 32 nm in thickness and can be stored under ambient conditions over weeks with no signs of degradation (peaks related to the formation of Sb2O3 or Sb2O5). This LPE strategy, which was initially developed for bP,44,45 has been one of the few top-down routes allowing isolation of FL-Sb without oxidation. Despite this, it has the disadvantage of generating flakes with poorly defined morphologies, incompatible with the preparation of dispositives, although very useful for other applications beyond electronics.
Following up on these works, we performed an extensive study on Sb LPE production, aimed to improve the lateral size distribution as well as the exfoliation yield. Note that due to the increment in the interlayer interactions in comparison to bP, yields were lower than 1% – a common result for 2D materials exfoliation. Thus, we carried out a systematic study on the experimental conditions, considering from the pre-treating protocols (manual grounding, dry and wet ball milling) to the solvent selection and exfoliation methodology (tip or bath sonication).42 We demonstrated that while NMP:water mixtures enhance the final yield, 2-butanol increases the dimensional anisotropy ratio (defined as the ratio between the length and height of the nanolayers) (Fig. 3G–I). Interestingly, FL-Sb obtained from 5:1 NMP:water mixture exhibits a lower oxidation degree probably due to the formation of a protective layer onto Sb flakes’ surface. Furthermore, when these Sb-based samples are compared in terms of hydrogen evolution reaction (HER) activity, the one obtained from 2-butanol exhibits better performance probably due to the irreversible formation of antimony oxide and the lack of a solvation protective shell.
Regarding 2D-As and Bi, their production was achieved with similar, and often the same, production methods of 2D-Sb. In example, shear force exfoliation using common kitchen blenders in aqueous media was employed to exfoliate pnictogens crystals, giving few-layer As, Sb, and Bi nanoplatelet.23 Besides, this method induced oxidation of the exposed surface and formation of Pn-oxides during the process. The same group, in a following study, achieved the production of low-oxidised and ultra-thin As sheets (2–4 nm) by LPE using NMP as solvent,46 as previously demonstrated for bP.15 Hang Qi et al. elucidated by DFT calculation the interaction effect of arsenene surface and solvents, to replace high-boiling point solvents and simplify 2D-As processing. Low-boiling point solvents such as THF, chloroform and cyclohexane were reported to have the best absorption energy/transfer energy ratio, and yielded slightly oxidised nanosheets with thickness between 33 to 49 nm.47 In a very interesting study, Wu and coworkers reported the production of the less thermodynamically stable α-arsenene (called black-arsenene (bAs) over the most famous bP). The researchers obtained layers of several micrometers of lateral dimensions by μME, and demonstrated that 2D-bAs possess high anisotropies along AC and ZZ, directions in its conductance, carrier mobility, and thermal conductivity.48 In the case of bismuthene, bulk Bi is harder to exfoliate because of its greater interlayer interactions. Indeed, to the best of our knowledge, bismuthene μME exfoliation has not yet been reported. Therefore, novel assisted exfoliation methods have been developed, besides common LPE.49 In one example, a new exfoliation strategy combining water exfoliation with H2O2/H2SO4 intercalation was developed.50 Sulfuric acid intercalation occurs by means of hydrogen peroxide gas formation, which expands Bi structure, facilitating the acid intercalation. Furthermore, the nanosheets (average lateral size 735 ± 297 nm and thickness of 6.7 ± 3.2 nm) were purified by solvent exchange with NMP.
Table 1 summarises some of the most typical bottom-up approaches for 2D-Pn production.
Morphology | Size; thickness (nm) | Preparation methods | Ref. |
---|---|---|---|
P | |||
Nanosheet | ∼1.5 micrometers (0.85 nm) | μME | 41 |
Nanosheet | ∼100–350 nm (3.5–5 nm) | LPE | 24 |
Nanosheet | ∼100 nm–3 μm (0.5–0.7 nm) | LPE | 15 |
Nanosheet | 100–200 nm (1–15 nm) | Solvothermal | 32 |
Nanoribbons | 75–1000 μm (4–50 nm) | Intercalation of lithium ions in ammonia based solvent | 51 |
As | |||
Spherical nanoparticles | ∼67 nm | Colloidal | 52 |
Nanoparticles | 30–164 nm | Colloidal | 53 |
Nanosheets | 100–900 nm | Liquid-phase shear exfoliation | 23 |
Nanosheets | Several micrometers (2.9–3.5 nm) | μME | 48 |
Nanosheets (NS) | NS: Several micrometers (3 nm) | LPE | 54 |
Nanodots (ND) | ND: 100–350 nm | ||
Nanosheets | Several nm (5–12 nm) | LPE | 46 |
Nanosheets | 100–1050 nm (33–49 nm) | LPE | 47 |
Sb | |||
Nanoflakes | 20–40 nm | Colloidal (microwave-assisted reduction using zinc powder) | 55 |
Nanoparticles | ∼ 2.8–6.6 nm | Colloidal (reduction with NaH) | 56 |
Irregular and spherical nanoparticles | ∼24.2 nm (13.1–23.5 nm) | Colloidal (hot-injection procedure) | 57 |
Diameter of ∼4.6 nm | |||
Nanosheets | Several micrometers (below than 100 nm) | μME | 43 |
Nanorods | 200–300 nm (50–80 nm) | Colloidal (reduction with oleylamine) | 58 |
Nanosheets | Few micrometers (less than 20 nm) | LPE (sonication in a mixture of 4:1 isopropanol/water | 25 |
Quantum dots | ∼2.8 nm | LPE (ultrasound probe sonication) | 59 |
Nanosheets | 40–300 nm (2–10 nm) | LPE (wet-ball milling in 2-butanol and liquid exfoliation using sonication tip in 4:1 NMP/H2O) | 42 |
Spherical nanoparticles | 34–42 nm | Colloidal (reduction using NaBH4) | 60 |
Quasi-hexagonal nanosheets | 0.5–1 μm (∼46 nm) | Colloidal (hot-injection method using alkyl phosphonic acids) | 38 |
Nanosheets | ∼3 μm (less 2 nm) | Pressurized alloying exfoliation | 61 |
Hexagonal nanosheets | 0.5–1.5 μm (5–30 nm) | Colloidal (hot-injection method) | 39 |
Hexagonal nanosheets | ∼6 μm (4–20 nm) | Colloidal (continuous-flow procedure) | 40 |
Bi | |||
Spherical nanoparticles | 11–22 nm | Colloidal (hot-injection procedure) | 62 |
Nanowires and nanoflowers nanoparticles | ∼20 nm | Colloidal (solvothermal method) | 63 |
Nanoparticles | 40–80 nm | Colloidal (using hexadecyl amine as reducing agent) | 64 |
Spherical nanoparticles | ∼4 nm | Colloidal (with ocatadecylene/oleic acid) | 65 |
Nanoparticles (NP) | NP: 10–50 nm | Colloidal (reduction reaction using NaH2PO2·H2O) | 66 |
Nanobelts (NB) | NB: several μm (10–100 nm) | ||
Spherical (S), cubes (C) and triangular (T), and nanobelts (NB) nanoparticles | S: 20–200 nm of diameter | Colloidal (polyol process) | 67 |
C: 60–80 nm of edge length | |||
T: 200–500 nm | |||
NB: ∼80 μm (0.6 μm) | |||
Quasi-hexagonal nanosheets | 100–500 nm | Colloidal (hot-injection method using alkyl phosphonic acids) | 38 |
Hexagonal nanosheets | 0.5–7.5 μm (below 20 nm) | Colloidal (hot-injection method) | 68 |
Nanosheets | ∼20 nm (2 nm) | Ionic liquid assisted exfoliation | 69 |
Nanosheets | ∼0.8 μm (∼4 nm) | Sonochemical exfoliation | 49 |
Nanosheets | 735 ± 297 (6.7 ± 3.2 nm) | Acid intercalated exfoliation | 50 |
Nanosheets | 50–200 nm (∼9 nm) | Electrochemical exfoliation | 70 |
Irregular shape nanoparticles (I), quasi-hexagonal nanosheets (H) and spherical nanoparticles (S) | I: 80–120 nm | Colloidal (solvothermal procedure using hydrazine) | 71 |
H: 700–900 nm (7–12 nm) | |||
S: 10–19.4 nm | |||
Dots (D), nanoplates (Np), nanorods (Nr) | D: 30–45 nm | Colloidal | 72 |
Np: ∼50 nm to ∼100 nm | |||
Nr: ∼20 nm × ∼80 nm |
To date, one of the few examples of controllable top-down approach is represented by the achievement of phosphorene nanoribbons (PNRs).51 Howard and co-workers, by means of a LPE approach, obtained monolayer PNRs with nanometric width (4–50 nm) and length up to 75 μm, corresponding to an aspect ratio up to 1000. The production follows a first step of bulk bP intercalation with metallic lithium (detailed description of this method will be found at paragraph 3.2 covalent functionalization, vide infra) followed by gentle shaking and separation by sedimentation. The authors also suggest that the breaks occur on longer P–P bonds in the zigzag direction, due to increased strain between intercalated and non-intercalated zones.51,73 PNRs were further employed to produce hybrid solar cells, acting as an effective charge-selective interlayer by enhancing hole extraction from polycrystalline perovskite to the semiconductor, as predicted in several theoretical investigations.74–76
As chemists, we consider that the solution for producing large anisotropic 2D layers of heavy pnictogens will come from bottom-up wet-chemical approaches.
Several examples of colloidal approaches controlling size and morphology are present in literature. In the case of pnictogens, generally Pn(III) salts and the common reducing agents for metallic nanoparticles synthesis (e.g.: NaBH4, NaH, N2H4 oleylamine, and dodecylamine)77,78 have been employed to obtain of As,53,79 Sb56,57,79 and Bi nanoentities.62,67,79Table 1 compiles some selected examples of these syntheses. Among these, we would like to highlight a study exemplifying the great potential of chemistry for on-demand controlling size and morphology nanomaterials. Buhro and co-workers reported the controlled synthesis of metallic β-Bi spherical nanoparticles (<25 nm), hexagonal nanoplatelet (ca. 100 nm) and nanoribbons (<50 nm width and >2 μm length) from a colloidal point of view, exclusively.72 We envision that this pioneering work represents a starting point for the synthesis of larger and thinner Pn-based 2D nanomaterials.
Indeed, the first wet-chemistry colloidal synthesis for 2D-Sb dates from 2019. Large hexagonal crystals of Sb exhibiting lateral sizes up to 1.5 μm and thicknesses ranging from 5 to 30 nm were obtained by controlling the anisotropic growth in a colloidal mixture of organic solvents.39 More in detail, the synthesis of Sb-based hexagonal crystals consists of a two-step hot-injection approach. Firstly, the precursor is prepared by dissolving antimony chloride into a dodecanethiol (DDT) and 1-octadecene (ODE) mixture at 110 °C for 2 h under vacuum conditions, and then heat up to 150 °C to trigger the reaction. Afterward, the precursor is injected into a oleylamine (OA) and ODE mixture at 300 °C, giving rise to the formation of the hexagonal crystals.39 Less than a year later, in 2020, the same authors reported a modified protocol that permits the synthesis of both Sb and Bi well-defined crystals.38 From these two pioneering works, our group set about optimizing the synthetic parameters to produce high-quality few-layer Sb hexagons (Fig. 4A).40 The accurate selection of the initial conditions allow the tuning of size from 200–300 nm to 2–3 μm, and the systematic analysis of the synthetic conditions revealed the tremendous influence of the solvent used on their final surface oxidation, being chloroform the most appropriate one for keeping unoxidized surfaces (Fig. 4B–K). Furthermore, by designing a continuous-flow synthesis reactor we achieved the production of high-quality few-layer Sb hexagons in large quantities (ca. 1 mg h−1 (Fig. 4L)). Additionally, we have tested the electronic properties of our colloidally obtained Sb crystals, which indeed compete favourably with those produced by micromechanical exfoliation. These results highlight the role of colloidal-based synthetic methods to produce a large number of high-quality Sb crystals with the desired electronic properties. Later on, Torres et at.68 presented another synthetic protocol for the isolation of hexagonal Bi micro-scale crystals under milder conditions than those reported for Sb. These Bi-based particles exhibit surface oxidation and present excellent mechanical and electrical properties that can be employed in NADH sensors, where Bi material acts as an electrocatalytic platform owing to a high charge transfer during donor–acceptor processes.
Fig. 4 Schematic representation of the synthetic procedure (A). Summary of the experimental parameters influencing the reaction (B). AFM profile of hexagonal Sb nanosheets with overlaid thickness profile (5 nm height over 2.8 μm diameter). Scale bar of 1 μm (C). Raman mapping of A1g (150 cm−1) intensity with optical micrograph given as inset (D). Raman signal comparison of bulk antimony and Sb hexagonal nanosheet (E). Typical XPS line spectra of Sb 3d 5/2 and 3/2 region for Sb hexagonal nanosheets (under environmental conditions) showing contributions from both metallic and oxidised Sb components. Individual contributions from the fitting are highlighted (F). HAADF STEM image of an individual nanosheet (G). Coloured high-resolution STEM-HAADF image to emphasise the amorphous edge surrounding the particles. Inset shows the FFT demonstrating the crystallinity of the material. Scale bar of 5 nm (H). EEL spectrums of FLA hexagon dispersed in chloroform (black) and dispersed in IPA (red) (I). Typical XPS line spectra of FLA hexagons synthesised by continuous flow procedure dispersed in chloroform (J). Typical XPS line spectra of FLA hexagons synthesised by continuous procedure dispersed in IPA (K). Schematic representation of continuous flow synthesis (L). Figures adapted with permission from ref. 40. |
As a summary of this part, we would like to confront the efficacy of Pn production methodologies. Table 1 summarises the main morphological characteristics of Pn produced by top-down and bottom-up approaches, highlighting the importance of colloidal synthesis as the most efficient and reproducible approach for the production of heavier 2D-Pn.
In this framework, in collaboration with Prof. Coleman's group, we investigated whether it was possible to use new solvents capable of promoting exfoliation and at the same time preventing bP oxidation.15 For instance, CHP was found to be a good candidate to exfoliate bP under ambient conditions, allowing the preparation of suspensions of stable bP flakes for days (Fig. 5), much longer than the first observation of ca. 1 hour of stability for μME flakes.81 Motivated by this result, sodium cholate, was also employed as surfactant due to its well-known role as an exfoliating agent in water-based mixture.6,83 Nevertheless, besides bP exfoliation can be carried out successfully, the reported stability is much lower in comparison to that obtained with CHP. Thus, it was hypothesised that the stabilisation relies on the ability of CHP to form a solvation shell on top of the bP surface. Keeping this in mind, the solvent/surfactant selection must cover two important aspects: (i) be able to exfoliate and prevent reaggregation of the sheets, as it was usually thought for 2D materials in general; (ii) protect the surface from oxygen interactions by forming a compact protective layer (solvation layer), avoiding further degradations. Hence, this fact limits the number of solvents or surfactants that can be employed for the successful preparation of bP suspensions.
Fig. 5 bP flakes obtained by LPE employing CHP as solvent: mean Raman spectra (λexc = 633 nm) summed over the region of an as-prepared sample as a function of exposure time. Spectra are normalised to the silicon peak at 521 cm−1. Inset: Raman A1g intensity map of the sample region (A). Sequence of AFM images of the same sample region of an as-prepared sample, and after 1, 4 and 11 days of exposure to ambient conditions, respectively (scale bar, 600 nm) (B). TEM images of the same flake deposited from a freshly prepared dispersion and after 16 days (C). Figure adapted with permission from ref. 15. |
As the rapid oxidation of bP is one of the major limitations for the characterization of this material, with the group of Prof. Hirsch we developed a methodology based on statistical Raman spectroscopy (SRS) to monitor the degradation of few-layer bP.45 Employing the influence of bP anisotropy on A1g/A2g Raman band (indicative of the oxidation state),15,84 we compared SRS with AFM measurements. Data were collected every 24 h, showing clear evolution of Raman bands ratio along time, more pronounced after 72 hours. The development of A1g/A2g ratio distribution as a function of time allowed to follow the environmental degradation of bP, showing an exponential decay trend of the Raman band ratio intensity. Additionally, the same study also demonstrated that visible light can promote a faster degradation process. In addition, we were able to demonstrate the important role played by both flake thickness and lateral dimensions in bP oxidation kinetics, an important aspect to consider when comparing results.
Once understood how to control the bP degradation, this oxidative behaviour was employed as a soft chemical exfoliating tool to reach the monolayer bP. Indeed, by exposing micromechanical pre-exfoliated bP under ambient conditions, followed by washing with deoxygenated water, the bP thickness can be reduced layer-by-layer following iterative cycles. It is worth mentioning the quality of the obtained flakes is good enough to prepare FET showing competitive mobility values.85 Furthermore, to achieve high-quality unoxidized few-layer bP by LPE it is recommended to work under inert conditions, and preferably using NMP as a solvent and an Ar-filled glove-box (<0.1 ppm O2 and <0.1 ppm H2O), avoiding oxidation and decomposition of the catalyst.15 Afterwards, to avoid the presence of NMP–which precludes a proper characterization of the flakes by AFM, among other fundamental techniques–the FL-bP can be transferred to THF by sequential ultracentrifugation and re-dispersion using increasing centrifugation speeds, leading to stable dispersions with <0.01 wt% of NMP, and absence of oxidation, evaluated by the A1g/A2g > 0.4 intensity ratio statistics (average 0.79).86
Fig. 6 Calculated frequencies of Raman-active vibrational modes in antimonene (a), and different antimony oxides (b–e). Except for (b), the height of the bars indicates the calculated Raman activity in logarithmic scale (A). Electronic band structures and density of states were calculated using the hybrid functional HSE12 and the inclusion of spin–orbit interactions (SOI) for two different Sb2O2 structures and Sb2O3 monolayers. Gray dashed lines are the results without SOI and are almost congruent with the bands with SOI. The zero of energy is set to the Fermi energy (B). Figure adapted with permission from ref. 88. |
We hypothesise that the formation of a superficial antimony oxide layer, different to what was demonstrated for bP,85 can protect the material from further oxidation. Moreover, these layers are semiconducting, with direct and indirect band gaps between 2.0 and 4.9 eV. Based on these calculations and the experimental data, we believe that the formation of layered heterostructures of semimetallic FL-Sb coated by semiconducting 2D Sb2O3 layers can naturally be formed (Fig. 6B).89 In addition, the frequencies of Raman-active vibrational modes of these species were calculated, providing clear fingerprints for the identification of antimonene oxides, and showing good agreement with our experimental findings. Moreover, these studies rule out the formation of antimonene oxides consisting of the formation of SbO bonds [type (I)], leading in turn, to oxygen atoms incorporated into the antimonene sheet [type (II)].89
Along this front, we studied the photothermal oxidation in antimonene. For this we used μME Sb-based nanosheets using viscoelastic adhesive film with high sticking coefficient, confronting the tape with a second piece of adhesive film while pressing and rapidly releasing from each other in an iterative process. This exfoliated material consisted of polygonal shapes with smooth surfaces and sharp edges, showing atomic terraces of ca. 1 nm and thickness in the range of 15 nm. Interestingly, a linear temperature dependence of the position of the Raman modes was observed, explained by the phenomenon of anharmonic lattice vibrations mediated by phonon–phonon interactions (Fig. 7A and B). We extracted the first-order temperature coefficients for the A1g and Eg modes χ = −0.027 and χ = −0.025 cm−1 K−1 (Fig. 7C), respectively, and estimated a thermal conductivity value of ca. KSb = 90 W m−1 K−1. For that, we fixed the laser power to 0.88 mW, in order to avoid laser-induced oxidation. A phenomenon that starts at 593 K leads to the appearance of the Raman signals associated with the surface formation of the α-phase of antimony oxide (α-Sb2O3). This observation falls in line with the reported low lattice thermal conductivity of antimonene and suggests a high figure of merit for application in thermoelectric devices, being described by a combination of laser power- and wavelength-dependent studies with a numerical heat transfer model (Fig. 7D–F). Moreover, by adjusting the laser power and using a spatially resolved Raman mapping, it is possible to control the surface photo-oxidation of antimonene (Fig. 7G–H) paving the way for the experimental realisation of arbitrary heterostructures of Sb2O3/antimonene. These exotic structures exhibit great potential in optoelectronics, promoting the cytotoxicity of cancer cells and even improving the catalytic activity towards different reactions.16
Fig. 7 Raman spectra of Sb nanosheets (Sb-NS) measured as a function of temperature from 298 to 633 K (A). Schematic diagrams of Raman active modes. Green and blue arrows indicate the direction of the atomic vibrations (B). Temperature dependence of the Raman peak positions for the A1g (green squares) and Eg (blue circles) modes (C). Raman spectra of Sn-NS measured as a function of excitation laser power (λexc = 532 nm) from 0.14 to 14 mW (D). Power coefficients, χp, for both two modes (green squares and blue circles for A1g and Eg, respectively) are extracted from the slope of the linear fits (solid lines) (E). Temperature of the probed Sb-NS as a function of laser power, was estimated using both calculated power and temperature coefficients (F). AFM image of an isolated Sb-NS before and after spatially-resolved mild oxidation using 532 nm laser at 3.9 mW for 10 s (G), height profile along the dashed red and green lines before and after laser-induced oxidation, respectively (H). Figure adapted with permission from ref. 16. |
Fig. 8 Schematic representation of the general non-covalent functionalization approach of micromechanically exfoliated/grounded bP by the use of perylene diimides (PMI) with three different peripheral moieties containing aromatic groups (A). DFT-optimised structures highlight the interaction between the different PDIs and the bP surface (B). Normalised mean Raman spectra of the bP-PDI hybrids showing enhanced intensities for each of the perylene bands. The measured flakes exhibit the same heights in order to ensure the correct comparison of the intensities (C). AFM images of the μME bP flakes after hybrid formation with PDI R3 (D). Statistical Raman Microscopy of the A2g bP (E) PDI representative Raman modes (1383 cm−1) modes of bP-PDI R3 (F). XPS spectra of Sb 3d peak for pristine (G) and functionalized (H) Sb samples. Numbers identify the different components: 1 (Sb 3d5/2), 2 (oxidised Sb 3d5/2), and 3 (O 1s). Peaks at higher binding energy values are the Sb 3d3/2 components. The black dots are experimental points and the red line is the result of the fitting. Grey lines correspond to the different components used and the background. Top and side views of the optimised geometries of PDI core on single-layer Sb. The electron density difference between the PDI-antimonene and the isolated molecules and antimonene is also shown in the side view. Images adapted with permission from ref. 87 and 99. |
Analogous results were demonstrated by other groups keeping in mind the typical donor–acceptor Lewis acid-base interaction.100–102 For instance, acid cations such as Ag+, Al3+ and Ga3+ salts have been successfully employed to increase the stability of bP under atmospheric conditions, preserving the electronic properties.103–105
Besides these pioneering contributions mainly based on bP, the research on non-covalent functionalization of the other Pn's members is currently under investigation. In 2017, we performed the first study on non-covalent functionalization of μME and LPE Sb flakes with PDI molecules (Fig. 8I).87 Scanning photoelectron microscopy cooperatively with DFT calculations suggest a much stronger interaction of Sb-PDI hybrids in comparison to bP-PDI ones, resulting in a 2-fold larger charge-transfer process, demonstrating the role of non-covalent functionalization on the electronic properties. Recently, the supramolecular functionalization of LPE Sb flakes with oligonucleotide has been carried out allowing the first steps to DNA sensor development.106 Recently, Rao and co-workers have applied pure inorganic acid-base Lewis interactions with different moieties to enhance Sb and Bi stability.107 Thus, non-covalent functionalization arises as an effective tool for Pn protection, keeping intact the crystalline structure and preserving the electronic properties.
Fig. 9 Schematic representation of the sequence adopted to perform the covalent functionalization of bP (A). Generally, pristine bP is intercalated with an alkali metal in the solid state under controlled heating and afterwards, the activated bPIC is dispersed in THF and reacted with an electrophilic trapping reagent, usually a alkyl iodide (B). Mean Raman spectrum of methylated NaP4 highlighting the different wavenumber regions (C). 31P-MAS solid state NMR spectrum of methylated BP as a function of Na:P ratios (D). Correlation of the functionalization degree determined by quantitative 31P-MAS solid state NMR spectroscopy to the Raman intensity ratio of the C–H and P–C vibrational mode versus the A2g mode of bP (E). Representation of lattice opening, according to the proposed reaction mechanism, of bP upon covalent modification with methyl iodide (F). Figures adapted with permission from ref. 112 and 114. |
Firstly, the bPICs formation was investigated by in situ XRD and Raman spectroscopy, respectively showing change from AB to AC stacking for intercalation compounds, as well as a series of novel Raman active modes, in agreement with DFT calculations.73 Starting from that base, we demonstrated the feasibility of bP functionalization with organic molecules through the reductive route (Fig. 9B).112 To get insight into the reactivity of bPICs, the reaction was followed in situ by Raman spectroscopy, evaporating in ultra-high vacuum conditions the hexyl iodide molecule in the reactor. The evolution of Raman spectra showed the arising of new active modes below 500 cm−1 (145, 210, 270, 320, 405 cm−1) (Fig. 9C–E). Additionally, through DFT calculations the effect of the functionalization on bP was evaluated. Interestingly, and contrary to what was expected (i.e. the formation of phosphonium sites), the formation of P–C bonds causes the lattice opening due to the cleavage of some P–P bonds (Fig. 9F) (observed by structure relaxation and by the increasing of the length of P–P bond close to P–C bond, from 2.26 to 2.83 Å). This process was demonstrated, by using a combination of several spectroscopic techniques, to be reversible after thermal-induced retrofunctionalisation.
Regardless of the covalent functionalization method used, it is necessary to quantify the degree of functionalization to have control over the properties of the material. Generally, destructive techniques such as elemental analysis (EA) or thermogravimetric analysis (TGA) are often employed, however, both require relatively high quantities of the solid material and have several limitations. To solve this situation, we developed a simple quantification method based on statistical Raman spectroscopy (SRS), correlated to quantitative magic-angle-spinning 31P solid-state NMR (31P-MAS NMR) as a reference technique.114 We discovered that the evolution of C–H (2900 cm−1) and P–C (645 cm−1) signals in comparison to A2g bP one (446 cm−1), expressed as IC–H/IA2g and IP–C/IA2g ratios, directly depends on the functionalization degree (analogously to the ID/IG ratio employed in graphene chemistry).110 It is important to remark here that the use of statistical Raman spectroscopy (SRS) allows for a simple and quick characterization of bP materials, not possible to achieve before without the use of more complex techniques. Indeed, we strongly recommend the use of SRS for 2D-Pn materials characterization since single-spectra analysis could induce misinterpretations. Thus, mapping large area surfaces, measuring, and analysing in an automatic way hundreds (or thousands) of spectra, will provide a better understanding of the material quality, avoiding possible bias. Despite the good results on bPICs functionalization employing alkyl iodide salts, not every reagent can be used to functionalize bP intercalation species. Aimed to improve the low yields shown by the neutral route with diazonium salts, we investigated the applications of these reagents to the reductive route. Surprisingly, after the reactions, bP was not showing the presence of functionalization. On the other hand, the material presented drastic structural evolution, with loss of crystallinity and formation of amorphous red phosphorus structures, where probably this process is promoted by intermediate radical centres on the P-lattice.115
One of the most promising fields of application for Pn is (opto)electronics, especially in the case of bP, since it presents a layer-dependent bandgap. The development of bP-based field effect transistors (FETs) has always gone hand in hand with different strategies to preserve the devices from environmental degradation. Along this front, the noncovalent functionalization stands-out as one of the most promising ones. Indeed, a significant surface passivation can be obtained by using optimised tailor-made PDI molecules endowed with aromatic end-groups, allowing the creation of the first environmentally stable hybrid bP FETs device showing a hysteretic charge balance behaviour. The preservation of the electronic properties of bP is clearly reflected in the values of charge carrier mobilities comprised in the 130–140 cm2 V−1 s−1 range corroborating that the use of these PDIs is optimal to preserve the electronic properties of bP (Fig. 10A–D).96
Fig. 10 Topography AFM image of the electrically investigated bP flake before processing. The height profile is shown as an overlay in the image (A). Microscope image of the processed bP field-effect transistor. The current is sent through the source and drain contacts while the 4-probe voltage is measured between the contacts 4p1 and 4p2 (B). 4-Probe current–voltage (I–V) measurements on a bP field-effect transistor for various gate voltages (each curve is averaged over 5 consecutive measurements). All I–V characteristics are perfectly linear (C). From the slopes the gate-dependent conductance is obtained and displayed in (D). The gate-voltage sweep presents a hysteresis with two branches (blue and red curves) with a seamless closure at VG = 0 V (D). Catalytic studies by employing Pn materials. Experimental evidence and proposed mechanisms for bP, Sb, and superacid triflic acid (HOTf) catalysed-alkylation of nucleophiles with esters in ionic liquid (E). Plausible mechanism for the bP and low valence Fe-catalysed atom-transfer radical addition (ATRA) and polymerization (ATRP) reactions (F). Electrochemical characterization in terms of HER for Sb-based materials obtained through different sonication methods. LSV curves of the different Sb-based samples, Nafion modified glassy carbon and platinum blank (G). Tafel slope values (H) and overpotentials required for achieving 10 mA cm−2 calculated from LSV data (I). CV curves recorded after LSV measurements of Sb-BuOH (J) and Sb-NMP (K). The study of the parameter affecting the formation of the sodium/black phosphorus intercalated (bPIC) phase via solid-state reaction can provide fundamental details towards sodium-ion batteries based on Pn material electrodes (L). Figure adapted with permission from ref. 86, 44, 42, 99 and 113. |
As previously shown, 2D-Pn exhibit a large chemically active surface and pronounced ability to adsorb and stabilise unsaturated organic molecules through van der Waals interactions. Owing to the control and stability against oxidation achieved on bP and Sb production we were able to investigate their potential for catalytic applications in organic chemical reactions for the first time. In 2019, we demonstrated how few-layer bP and Sb can catalyse the alkylation of soft nucleophiles with esters (Fig. 10E and F).11 The materials, produced by LPE and stabilised with bmim-BF4 ionic liquid, exhibited good catalytic activity for alkylation of soft nucleophiles with alkyl esters, with good performance for aromatic substrates. In addition, it was shown that the employment on Pn allows mild reactions conditions, avoiding superacid-mediated alkylation and permitting alkylation with substrate containing acid-sensitive moieties.
Moreover, in the particular case of bP, the availability of the P surface atom orbitals for external reactants together with the cooperativity of the atomic network and the possibility of reversible lattice opening (i.e. breaking temporarily P–P bonds) to exchange one electron,112 would make, in principle, this 2D material a potential catalyst for radical reactions. In a detailed study with Leyva-Perez and co-workers, we demonstrated that FL-bP catalyses with extraordinary activity different radical additions to alkenes with an initial turnover frequency (TOF0) up to two orders of magnitude higher than other metal complex catalysts at room temperature.86 Moreover, this value was almost doubled when sodium BIPCs were employed. Comparison with other nanomaterials and their reduced forms (including graphene intercalation compound KC8 and Fe0vs. Fe2− complexes) indicates a marked increase of catalytic activity when the catalyst is negatively charged. These results represent a very promising starting point for the development of novel 2D radical catalysts based on p-block elements, and also reveal the important role played by the reactivity of these materials in their interaction with other substances, a chemical behaviour clearly different to that of graphene.
2D-Pn also demonstrated promising optical properties. Indeed, both Sb and Bi nanosheets were reported having nonlinear optical response, nonlinear refraction, and nonlinear scattering, to be potentially employed on photonic devices, laser protection devices, and all-optical Kerr switches. Example of this is represented by the previously mentioned silane-functionalized Sb nanosheets. The covalent functionalization improved their dispersibility in polymeric matrix, to which the material was covalently bonded during reaction. The produced gel glass showed strong and ultra-broad-band OL performance at 532–2150 nm.118 2D-Bi nanosheets dispersed in NMP, were dropped onto a gold mirror, exhibiting a nonlinear absorption coefficient of −3.9 × 10−10 mW−1, and demonstrated the potential to substitute semiconductor saturable absorber mirrors, especially in the NIR region.50
If there is a field that has received a great deal of attention in recent years, it is energy. In this sense, 2D materials, and 2D-Pn in particular, have several properties that make them especially interesting. With respect to energy conversion, Sb has been employed as electrocatalysts for water splitting, with special focus on hydrogen evolution reaction (HER) in acid media.23 For that, Sb-based materials obtained through LPE using different solvents and wet-ball milling processes have been obtained. Interestingly, we discovered that the preparation protocol triggers different oxidation degrees on the final materials, which results in marked differences in terms of HER performance. Indeed, the higher the surface oxidation, the better obtained overpotential values, and Tafel slopes. This is particularly the case for the samples prepared using BuOH, which exhibited better exfoliation and anisotropic ratio yielding a large number of edges and electroactive sites (Fig. 10G–K). This behaviour seems to also be related to the irreversible formation of superficial antimony oxides.42
Last but not least, concerning energy storage, 2D-Pn have been postulated as excellent electrode materials for Lithium Ion Batteries (LIBs) and Sodium-Ion Batteries (SIBs) because their 2D structures enable fast ion diffusion and easy accessibility to redox sites.124–126 It is also very important to mention their potential as anode material for alloy-based batteries. Indeed, heavy Pn show higher theoretical specific and volumetric capacities compared to graphite, the most widely employed anode material to date.127,128 Their ability to generate reversible alloys is the key point for their use, permitting fast charge/discharge mechanisms. Moreover, 2D-Pn exhibit lower volumetric expansion, decreasing the technological problems that arise during anode charge.129 Along this front, we carried out a thorough analysis of the sodiation process of the solid-state synthesis and the structure of the resulting intercalated bP/sodium phase, establishing the relevant parameters that lead to a successful sodiation. This solid-state protocol reveals the thermodynamically preferred range for the bulk formation of the intercalated phase, which consists of alternating Na-filled and empty layers as well as small areas of stage 1 intercalated layers (Fig. 10L). This work opens a door towards a large-scale synthesis of Na-bPIC, one of the most promising materials for SIBs.
From the point of view of the biomedical application, the rich chemical diversity of Pn play a very interesting role, making each of these 2D materials suitable for complementary applications.130–133 For instance, phosphorene exhibits great ROS scavenger behavior and its degradation is effective in the treatment of neurodegenerative diseases like Parkinson, ELA or Alzheimer.131,134–136 Conversely, antimonene ability to produce ROS combined with its great photothermal conversion efficiency (PTCE) can be exploited in cancer therapy to induce cellular toxicity and tumor ablation.121,137,138 Arsenene was proved having antiproliferative effects on different cancer cells, especially on promyelotic leukemia cells.139–141 Moreover, bismuthene could be used in therapies against antibiotic-resistant bacteria, owing to its antimicrobial properties.130,142–145
Undoubtedly, one of the most important aspects in the future applications of 2D-Pn is the control over nanomaterials morphology. In this regard, it is particularly inspiring a recent achievement from Howard and coworkers, which showed the controlled synthesis of phosphorene nanoribbons (PNRs),51 predicted to combine flexibility with unidirectional properties of one-dimensional materials together with high-surface area and electron-confinement effects.74,146 PNRs were obtained after lithium intercalation of bP, and in a sequent article the group demonstrated the potential of these materials in inverted perovskite solar cells, drastically improving the devices performance. Furthermore, in the PNRs the electronic properties strongly depend on the morphology and width,5 as well as the number of layers. For instance, in the case of bP, while bulk material has a direct bandgap (ca. 1.5 eV), NRs exhibit an indirect band gap that could be semiconductor or metallic depending on the structure.75,146 Thus, we envision the isolation of a great variety on single- and few-layers pnictogen nanomaterials byway using heavy Pn intercalated with alkaline metals in a similar manner. Moreover, in the particular case of Bi, these exotic morphologies could give place to additional surface states of importance in topological insulators.147 Nonetheless, as demonstrated for bP, the alkali metals intercalation approach could help to overcome the difficult problem of exfoliation of heavy pnictogens, as well as represent an innovative method for their covalent functionalization. Indeed, we believe that the preparation of large, high-quality monolayer 2D-pnictogens will be tackled by means of new advances in the field of alkali-metal intercalation as well as novel molecular bottom-up approaches. This will bring new horizons to the implementation of bP-based technologies, and in the development of novel pnictogen-based heterostructures with potential, among others, in (opto)electronics and spintronic applications, as long as the environmental stability is maximised by suitable functionalization.
Although the covalent chemistry of 2D materials has been extensively investigated in recent years, its transfer to 2D-Pn is not obvious due to its marked chemical reactivity. Indeed, bP functionalization already lived a quiet development, but heavy pnictogens haven’t experienced a similar situation. Their semi-metallic and metallic character is the main limitation to their covalent chemistry. One possibility for the covalent functionalization of Sb consists of exploiting the hydroxyl group formed during exfoliation, as reported by Xie and coworkers.118 This could open the door to an approach similar to that shown by the chemistry of graphene oxide, where the functional groups on the surface were employed for further functionalization, without extra modification of the main material structure. Organic chemistry is rich in examples of –OH functionalization, thus reactions with strong electrophiles could be considered as functionalization pathways. Moreover, this approach could be common to the heavy pnictogens, anticipated by a controlled oxidation of the material to introduce reaction sites. On the other hand, the direct covalent functionalization of the neat element constituting the material remains an open challenge, and its development could pave the way for an innovative control of Pn properties, as well as a useful tool for the synthesis of covalent hybrid materials. Considering the large number of published contributions on the synthesis of antimony and bismuth chalcogenides (S, Se and Te), this objective could be pursued by analysing the organometallic chemistry of molecules containing S and Se, as it was developed for gold nanoparticles by using thiol and selenide derivatives.148 Similarly, these groups could interact with lone pairs of As, Sb and Bi to form covalent interactions with the 2D structure. In a like manner to bP and other 2D materials, the surface functionalization will lead to punctual modification of the oxidation state of the functionalized atoms, as well as inducing lattice-strain on the Pn surface, consequently affecting their electronic and optical properties.149 These effects are yet unknown and represent a completely open field. In this sense, we believe DFT calculations can help experimental researchers, predicting the effect of the described modification on Pn properties, guiding the synthetic efforts in a rational way.150 Not of secondary importance, chemical functionalization could open the doors to the development of new functional materials and hybrids, including 2D–2D heterostructures, with a wide range of applications in electronics, nanomedicine and optics.
Finally, one of the aspects that highlights the importance of the chemical approach is the large limitations in the production of heavy 2D-Pn, which makes bottom-up approaches the only solution. In particular wet-chemistry methods like the recently developed colloidal approach hold great promise for the large-scale fabrication of high-quality 2D-Pn compatible with applications in electronics and beyond. Along this front, some works reported the preparation of 2D hexagonal crystals of Sb and Bi, however, further work should be done in order to precisely control the surface oxidation, size, thickness, and morphology. The great amount of reports based on Bi nano-entities demonstrate the feasibility of colloidal synthesis for general Pn production, providing a plethora of chemical precursors, solvents and conditions to work on it. Most of these reports present the synthesis of spherical nanoparticles,151–156 but also in some cases other morphologies such as nanocubes,67 nanowires,67 nanohexagons,157 faceted,158 and ribbons,72 among others. Nevertheless, considering the intrinsic anisotropy of the Pn structures, in-plane chemical bonds vs. out-of-plane interlayer interactions, soft chemical methods appear as the most proper ones to achieve a fine tuning of the morphological aspects. For instance, considering gold as an example, anisotropic growth can be promoted by the so-called seed-mediated growth. In this process, the formation of 2D systems would take place by the reduction of metal precursors on top of already formed small seeds. Then, the presence of the indicated shape-directing agents (metal ions, halides, organic compounds, surfactants) will drive the rest of the work.159 Additionally, the compatibility of colloidal synthesis approaches with organometallic chemistry of Pn(III) cations in the initial reaction mixture could represent a pathway for the production of hybrids (either non-covalent or with covalent functionalization) in a one-pot straightforward procedure.
Summarising, as the preparation of large, monolayer 2D-pnictogens remains an open challenge, we are convinced that the future scientific and technological development of 2D-pnictogens will depend on the success of the new bottom-up methods, and specially in the colloidal routes. Likewise, we anticipate that two fields of research related to 2D-Pn will experience significant growth in the coming years: energy storage and biomedicine. Concerning the former, antimonene and bismuthene exhibit great potential as anode materials for both lithium- and sodium-ion batteries, even surpassing graphene, mainly due to the fast ion diffusion through their layers and the ability to intercalate alkali metals, something particularly relevant in the case of sodium. This pronounced chemical reactivity of 2D-Pn may be particularly beneficial in the case of biomedical applications, showing great potential for cancer therapy, theranostics, drug delivery systems, photothermal agents, or biosensing devices, to mention a few.
Overall, we hope that this feature article serves to highlight the importance of chemistry in the development of these emerging materials as well as to encourage further research on 2D pnictogens, opening the door for the development of exciting applications.
Footnote |
† These authors contributed equally to this work. |
This journal is © The Royal Society of Chemistry 2023 |