Francis
Albarède
*,
Chloé
Malod-Dognin
and
Philippe
Télouk
Ecole Normale Supérieure de Lyon, Université de Lyon, France. E-mail: albarede@ens-lyon.fr
First published on 14th September 2023
It has been proposed that gold purification by cementation could account for the low gold content of ancient Greek coinage from Attica and the Cyclades. In order to place new constraints on this suggestion, the concentrations of platinum-group elements (PGEs) and gold have been measured in 72 silver coins mostly from the Greek Archaic and Classical periods, but also from Rome, India, medieval Europe, and colonial Spanish Americas, by inductively coupled plasma mass spectrometry. A novel technique allowing these concentrations to be determined in silver coins is described. Variations are consistent with element position in the periodic table. The volatile elements Rh and Os are commonly at or below the detection level, which may reflect evaporation during smelting and cupellation. Ruthenium and Ir, which binary phase equilibrium experiments show to be insoluble in solid silver and gold, and soluble Pd and Pt, show variations in coinage consistent with these properties. The dichotomy of Ir/Au ratios is not consistent with Ir loss in gold during salt cementation (parting) and is better explained by the contrast between Au-rich and Au-poor ore districts. This contrast is suggested to reflect either regional differences or the variability of conditions during ore genesis, such as hydrothermal solution chlorinity.
Fig. 1 Position of platinum-group elements (in orange) and related Re and Au (in pink) in the periodic table. |
The abundances of one of the PGEs, iridium, are better known because Ir concentrations can be determined by instrumental neutron activation. Wood et al.7 suggested that Au and Ir concentrations in silver coins could be used, especially in conjunction with lead isotope compositions, as a provenance tool for silver coins and artefacts from the first millennium BCE and for the Sassanian and Byzantine empire. Pernicka6 nevertheless argue that gold parting confuses the Ir signal and therefore assessed that Wood et al.'s arguments are unfounded. The cementation problem therefore needs to be addressed through new observations on silver coinage. Because this dispute has important consequences in archeology, it warrants a more in-depth study of PGE and Au traces in ancient silver.
The purpose of the present work is to explore the potential of PGEs and Au as markers of silver provenance and metallurgy. The sources of silver can be related to relatively low-temperature and low-sulfur epithermal ore deposits typically associated with Au.8 In contrast Au and Cu are often precipitated from the higher-sulfur, higher-temperature hydrothermal fluids that are expelled from felsic magmas in subduction zones and continental collision sutures (porphyry coppers). The preference of the elements in question for the melt phase decreases in the order Re > Au > Pd > Pt > Rh > Ir ≥ Ru ≥ Os.9–13 Basalts and, in general, the whole oceanic and continental crust therefore are enriched in Re over Os with respect to their mantle source, which makes Os enriched in radiogenic 187Os. Platinum, Pd, and Au are enriched over the rest of the PGEs in Cu sulfides.14 Platinum-group elements and gold's boiling temperatures exceed 2800 °C, but Ru and Os are easily oxidized as RuO4 and OsO4, which evaporate at ca. 130 °C.15 The latter two elements will therefore be easily lost during silver smelting. The relative abundances of PGEs and Au hence hold some potential for identifying both silver provenance and metallurgic processes.
Overall, literature on PGEs in silver coins and artefacts is sparse and data quality is variable. Gold and iridium analysis by neutron activation analysis were successful for some coins and artefacts7,16–19 but many of them remained below detection limits.20 Early PGE analysis by LA-ICP-MS were apparently not successful enough to be reported.21 Over the last two decades, laser-ablation ICP-MS allowed some PGEs to be measured on depth profiles in silver coins22 but the detection limit in silver coins, in general on the order of a few tenths or a few hundredths of μg g−1, seems to be a limitation and only few studies, if any, have been dedicated to these elements.
Here we describe a new protocol for the measurement of Au and PGEs in silver and apply it to 72 coins of different ages (Ancient Greece, Rome, Gaul, 16–18th century AD) and from different localities (eastern and western Mediterranean Europe, South America, Mexico) with the expectation that the new data will contribute to the issue of silver produced during gold parting.
The hydrochloric 37% laboratory reagent grade and nitric >68% trace element grade acids were obtained from Fischer Scientific and home-distilled. The Thermo Scientific ICAP-RQ was tuned with Tune solution, Tune B (1 ng g−1 Li, Co, In, Ba, Ce, Bi, U) in 2% HNO3 and 0.5% HCl. Single element standard solutions with 1000 μg mL−1 concentrations were obtained from Alpha Aesar. Abrasive paper was from Presi, type M, P320.
Step | Reagent | Volume | Time | Hotplate |
---|---|---|---|---|
Cutting coins (200 mg with pliers) | ||||
Polishing | ||||
Cleaning | Distilled water | |||
Weighing | ||||
Digestion | 8 M HNO3 | 5 mL | Overnight | 120 °C |
Ultrasonic bath (optional) | 30 min | |||
Centrifuge 8000 rpm | 10 min | |||
Precipitate separation | ||||
Aqua regia digestion: solution 1 | Aqua regia | 3 mL | Overnight | |
Supernatant AgCl precipitation | 6 M HCl | 3 mL | ||
Centrifuge 8000 rpm and separate AgCl | 10 min | |||
Adding distilled H2O: solution 2 | Distilled water | 5 mL | ||
Solutions 1 and 2 ICP-MS analyses | 0.5 M HNO3 with In |
The supernatant was treated with HCl to remove Ag. This step is necessary because, PGEs being ultra-traces, Ag must be removed to avoid polluting and clogging the instrument with metal and keep the beam stable. Three mL concentrated, distilled HCl were added to the nitric supernatant, which produced an abundant AgCl precipitate. The solution was centrifuged at 8000 rpm for 10 minutes and the supernatant transferred into a beaker containing 5 mL of deionized water, which brought the total volume to 12.5 mL. This second step produced ‘solution 2’. Because of the volatility of some elements, such as Ru and Os, solutions were not fully evaporated to maximize the yield of the chemistry. The yields of this procedure were determined by analyzing Alfa Aesar standard solutions combined to reproduce the composition of the samples. A full procedural yield of 100 ± 2% was achieved for Rh, Ir, Pd, and Pt. The yields for Ru and Os were smaller, 75% and 56%, respectively, and the missing fraction of these volatile elements seems to have been lost during the digestion stage. The Au yield was 61% with the missing Au likely being lost during AgCl precipitation. All the yields were reproducible within ∼10% and a correction was applied to the final results. The consistency between the 1-sigma coefficient of variation of Au concentrations (91%) is consistent with the coefficients for Pd and Pt (84 and 114%, respectively), showing that the applied correction is valid.
The total blanks of the procedure are reported in Table 2 and the instrumental noise (or background noise) is discussed below.
Ru | Rh | Pd | Os | Ir | Pt | Au | |
---|---|---|---|---|---|---|---|
Chemistry blank (ng g−1) | 0.0000 | 0.0010 | 0.0015 | 0.0000 | 0.0000 | 0.0000 | 0.4209 |
Instrument blank (ng g−1) | 0.0002 | 0.0003 | 0.0012 | 0.0039 | 0.0002 | 0.0012 | 0.0334 |
iCAP-RQ ICP MS operating conditions | |
---|---|
Instrument parameters | |
RF power (W) | 1550 |
Nebulizer gas flow (L min−1) | 1.05 |
Auxiliary gas flow (L min−1) | 0.8 |
Cooling gas flow (L min−1) | 14 |
Hexapole bias (V) | −1.000198 |
Collision cell gas (mL min−1) | He at 5 mL min−1 |
CCT bias (V) | −20.49 |
Analytical parameters | |
Acquisition mode | KED, peak jumping, simultaneous pulse count/analog detector |
Dwell time/isotope (s) | System |
Channel per mass | 0.01 |
Number of repetitions/samples | 1 |
Sample uptake/wash time (s) | 3 |
Total acquisition time per sample | 120 |
The monitored isotopes are listed in the ESI.† The kinetic-energy discrimination (KED) mode, which uses a collision cell filled with helium gas, reduces sensibility but minimizes spectral interferences. In order to reduce blanks, the mass spectrometer was first rinsed with 8 M distilled HNO3 for 20 minutes. The procedural blanks at this stage are given in Table 2. The sample/blank ratio, both for PGEs and Au, were higher than 100, which show that the blank can be neglected compared to the amounts of PGEs and Au processed.
All samples and standard solutions were spiked with a 2 ng g−1 In solution as an internal standard to correct for instrumental drift. The data were acquired and processed using the Thermo Scientific Qtegra Intelligent Scientific Data Solution Software.
Standard limits of detection (LD) are shown in Table 2. However, in order to evaluate data precision, and, critically, the effect of blank subtraction, the simple expressions derived in the ESI† were used. The error amplification factors (f) and final uncertainties were calculated for each element. Precisions better than 2% were achieved for Rh, Pd, Pt, and Au (Table 4). The relative errors on Os and Ir (53 and 33%, respectively) were rather large but, given that PGEs and Au concentrations typically vary over several orders of magnitude, the data remain informative. Finally, the relative errors on Ru and Re were on the order of 100‰ and the data only give an upper limit for the concentration (limit of detection). Adjusting sample size, as long as permitted by the separation protocol, and dilution may help minimize errors.
Re | Ru | Os | Rh | Ir | Pd | Pt | Au | |
---|---|---|---|---|---|---|---|---|
a Blank signal > sample signal. b Limit of detection (in ng of element per g of silver). | ||||||||
Blank ng g−1 | 26 | 12 | 148 | 7 | 24 | 4 | 32 | 1885 |
Rel. error | 0.36 | 0.53 | 0.15 | 0.71 | 0.38 | 0.89 | 0.32 | 0.04 |
Sample ng g−1 | 13 | 3.33 | 213 | 5908 | 77 | 45405 | 11462 | 1311140 |
Rel. error | 0.5 | 1 | 0.12 | 0.024 | 0.21 | 0.01 | 0.02 | 0.002 |
Amplification factor | ||||||||
f meas | −1.05a | −0.4a | 3.27 | 1.001 | 1.44 | 1 | 1.003 | 1.001 |
f blk | −2.05a | −1.4a | 2.27 | 0.001 | 0.44 | 0 | 0.003 | 0.00 |
σ n /n | 1.06 | 0.96 | 0.53 | 0.02 | 0.33 | 0.009 | 0.02 | 0.002 |
LDb | n.d. | 0.02 | 0.02 | 0.02 | 0.04 | 0.02 | 0.05 | 1.4 |
The coins with their type, origin, and age are listed in Tables S3 and S4† and represent a selection of coins from around the ancient Mediterranean world, a few samples from the Indian kingdoms such as Gandhara, and more modern coins from medieval and post-medieval Europe, as well as colonial Mexico and Peru. Pb and Ag isotopic data are taken from ref. 24–26.
Fig. 2 PGE concentrations of the 72 silver coins normalized to concentrations in EH chondrites. Note that the order of elements on the abscissa reflects the order of columns in the periodic table from the Fe group (Ru, Os), to the Co group (Rh, Ir), the Ni group (Pd, Pt), and the Cu group (Au). Dashed line: McCreedy Cu-rich sulfide from the Sudbury mine, Canada.14 |
Osmium concentrations are in general very low and often below detection limit. The perspective of using 187Os/188Os as a tracer is therefore unpromising. Osmium is most likely lost during smelting and cupellation. This is supported by the lack of a strong correlation between Os and other PGEs + Au.
Correlations between the logarithm of the different variables are summarized in Table 5 and the slopes in Table S6.† Palladium and Pt are strongly correlated (r = 0.93) (Fig. 3, bottom). Correlations between Au and Pt (0.83), Ir (0.72), and Pd (0.76) and between Ir and Pt (0.74) (Fig. 3, top), Ru (0.77), and Rh (0.71) are significantly weaker, but still significant at the 95% confidence level. Some of the correlation coefficients are high because of some data being exceptionally high or low (e.g., Ir–Rh, Au–Pt), notably those on the samples from colonial Spanish Americas which are particularly poor in Ir. Iridium seems to be constant at low Ru and only correlates with Ru when the abundance of the latter rises above the chondritic Ru abundance.
Ru | Os | Rh | Ir | Pd | Pt | Au | |
---|---|---|---|---|---|---|---|
Ru | 1.00 | ||||||
Os | 0.49 | 1.00 | |||||
Rh | 0.45 | 0.24 | 1.00 | ||||
Ir | 0.77 | 0.46 | 0.71 | 1.00 | |||
Pd | 0.49 | 0.45 | 0.31 | 0.64 | 1.00 | ||
Pt | 0.56 | 0.50 | 0.38 | 0.74 | 0.93 | 1.00 | |
Au | 0.53 | 0.36 | 0.30 | 0.72 | 0.76 | 0.83 | 1.00 |
CV% | 773 | 168 | 18 | 74 | 22 | 28 | 8 |
Fig. 3 Plot of Pd (bottom) and Ir (top) concentrations vs. Pt. Note the different scales on the vertical axes. Color coding according to Table S3.† |
Gold is the least variable of all the elements (±100.08 or ±21%) followed by Rh (±52%), Pd, (±67%), and Pt (±89%). The strongest correlations observed, Pt vs. Pd (slope = 1.7), Pt vs. Au (slope = 1.6), and Ru vs. Ir (slope = 1.2) are defined with rather narrow uncertainties. The Pt/Pd ratios vary by a mere ∼30 percent, which shows the very coherent behavior of these two elements.
Binary phase Ag–M diagrams, where M stands for a PGE or Au, are reasonably well known from the metallurgical literature.31–39 Positive slopes of the liquidus and the solidus of Ag binary phase diagrams attest to solubility of PGEs in solid silver at high temperatures. This is the case of Au, Pd, and Pt, which, however, do not fractionate to a large extent between solid and liquid silver. In contrast, Ir and Rh form no solid solution with silver.
Binary diagrams between PGEs and Au are less well documented.40–43 As for silver, Pd and Ag do not fractionate between liquid and solid gold, while Pt is slightly more soluble in solid gold. Ir and Rh solubility has not recently been revisited but early experiments attest to the insolubility of these elements in both liquid and solid gold.44–46
Metallurgical data therefore show that PGEs react as pairs defined by their position in the periodic table: (Cu)–Ag–Au (group 11, a.k.a. coinage metals), (Ni)–Pd–Pt (group 10), and (Co)–Rh–Ir (group 9). Information on the (Fe)–Ru–Os (group 8) is scant beyond the fact that both elements are volatile. The Cu group is the least sensitive to redox conditions.
The present results are relevant to the conflicting interpretation of Ir concentrations in Sassanide and Byzantine coinage by Wood et al.,7 who support a silver source in the Taurus Mountain range of southern Anatolia, and Pernicka et al.,6 who claim that Ir variations reflect the effect of cementation. We have seen above that Pd and Pt are soluble in both silver and gold, whereas, as far as the still incomplete thermodynamics show, Ir and Rh are insoluble in either metal. Iridium should therefore be lost during gold parting and fractionated with respect to Au-soluble Pd and Pt. Given the high abundance of silver in silver coins, ratios such as Ir/Ag used by Wood et al.7 are, for all practical purposes, equivalent to Ir concentrations in weight percent. The remarkable dual trend observed in the present data when Ir/Au is plotted against Ir (Fig. 4) is essentially equivalent to Wood et al.'s7 Fig. 3 of log10(Au/Ir) vs. log10(Ag/Ir). A plot of log10(Rh/Au) vs. log10(Rh) (not shown) demonstrates similar relationships. The data show that Au-poor and Au-rich groups form at constant Ir contents. The gap visible in this plot is clearly created by a gap in Au concentrations and is independent of the Ir variations. These plots are just other pieces of evidence of the dual distribution of Au in Greek silver coinage and of a contrast between high-Au and low-Au metallogenic provinces. In these plots, Athenian coins form a well-defined Au-depleted upper group. Nevertheless, a few non-Athenian coins (Argos, Thasos, Jaen, medieval Rouen, colonial Mexico) belong to the same group of Au-poor silver as Athenian coins. Source Au depletion rather than human intervention best accounts for these relationships.
The dichotomy observed in the Ir/Au vs. Ir plot is most straightforwardly interpreted as reflecting an effect of higher Au solubility in brines of variable chlorinity.47–53 Again, Au depletion of southern Aegean ores may correspond to a contrast between southern and northern Greece. Variable conditions, such as depth of emplacement and infiltration of meteoric water during the genesis of silver ores may lead to a different role of liquid–vapor separation or to dilution of ore fluids by the water table. At this stage, we conclude that the case of salt cementation in Athenian mints6 is not supported.
Can PGEs and Au be used as a provenance tracer? In Athenian samples, Au concentrations are low and the Rh/Ir ratios vary within the rather narrow range of 12–35. As for Athens, some consistent behavior is observed but, given the destructive nature of the analytical technique, it is difficult to see a bright future for the use of PGEs and Au as a routine provenance tool. Colonial silver coins from Spanish Americas (Peru and Mexico) are also strongly depleted in Ir, Pd, and Pt, and, for Mexico, Au, which may or may not be due to losses at the amalgamation stage of the patio method. Potosi coins are depleted in Pt and Pd with respect to contemporaneous coins from Mexico, which may indicate different silver refinement procedures. For Potosi samples, whether Au contents below the detection limit are due to an analytical problem or to intentional extraction of Au from metallic silver is not known: the very small Au content of the replicated analysis of Poto D suggests that gold may have been extracted from silver.
Using the published Pb isotope data obtained on the same samples, we followed Wood et al.'s7 lead of a possible correlation between Ir contents and Pb model ages. Iridium does not correlate with Pb isotopic ratios, except weakly with 207Pb/204Pb (r = 0.58), nor with model ages or κ (232Th/238U) values. A weak correlation is observed between Ir and μ values (238U/204Pb, r = 0.53). These weak correlations suggest that high Ir contents signal a source in terranes located south of the Variscan front (see Fig. 4 in Blichert-Toft et al.54), probably in crustal slivers detached from the Gondwana continent and embedded in the recent (<100 Ma) Alpine collisions. Wood et al.7 are not incorrect when they suggest that Ir contents are potential provenance tracers, but the present work nevertheless suggests that the resolution of this tracer is only at the broad scale of tectonic provinces, not at the scale of individual mining districts.
The behavior of PGEs and Au define coherent groups corresponding to the four successive columns of the periodic table: (Fe)–Ru–Os (volatile), (Co)–Rh–Ir, (Ni)–Pd–Pt, and (Cu)–Ag–Au. Phase diagrams provided by metallurgy establish that elements from the Ni group are soluble in Ag and Au without major fractionation. Elements of the Co group are nearly insoluble in Ag and Au. Salt cementation of gold considered as a source of silver, notably for Athenian coinage, must be more sensitive to Ir and Rh fractionation than Pd and Pt. The data show that Au-poor and Au-rich groups form independently of Ir content variations.
It is concluded that parting does not account for the relationship between Au and Ir first demonstrated by Wood et al.7 Rather, this relationship reflects bimodal Au distribution of silver sources possibly inherited from regional conditions of ore genesis. Iridium, however, is not a helpful tracer of geographic provenance.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d3ja00112a |