Vanadium-based compounds with stable crystal structures and high capacities are promising cathode materials in aqueous zinc-ion batteries (AZIBs); nevertheless, the sluggish solid-phase diffusion kinetics of zinc ions and poor electronic conductivity have obstructed their application. Herein, this study proposes a synergistic engineering approach involving carbon and oxygen vacancies to improve the performance of VO2. Compared to VO2, VO2@C shows improved electron/ion transport kinetics due to carbon coating, oxygen vacancy, expanded lattice, and reduced grain size. This composite also offers improved structural stability and extra active sites, enhancing zinc-ion storage performance. The optimized VO2@C-350 composite electrode displays a remarkable discharge capacity of 391 mA h g−1 at 0.1 A g−1 over 100 cycles and maintains good cycle stability performance at 2 A g−1 for over 2000 cycles. Further analysis has identified that its reaction mechanism involves a co-intercalation/de-intercalation process of the proton (H+) and Zn2+. This innovative synergistic engineering approach can be implemented in other zinc storage materials to achieve efficient AZIBs.
The cathode is an essential component in determining the energy density and cycle life of AZIBs. Various cathode hosts have been developed by researchers, including Prussian blue analogs (PBAs),10 Mn-based,11 V-based,12 and organic compounds.13 Cathode materials containing vanadium have gained significant attention due to their diverse crystal structures and valence states.14–16 These materials possess remarkable specific capacity, exceptional rate capability, and long-lasting cycle life. Among these, B-phase vanadium dioxide (VO2) is noteworthy for its one-dimensional tunnel structure formed by corners and edges shared by VO6 octahedra, which supports the intercalation and delamination of Zn2+.17,18 However, VO2 frequently faces issues such as sluggish solid-phase diffusion kinetics of zinc ions, poor electronic conductivity, and structural deterioration upon repeated ion (de)intercalation, leading to poor rate performance and a rapid decrease in capacity.19,20 To date, numerous high-efficiency strategies have been suggested to tackle these issues. To improve the electronic conductivity and structural durability of VO2, highly conductive carbon substrates such as graphene,21–24 carbon cloth,25 carbon fiber,26 and carbon coating layer27–30 have been utilized. Oxygen vacancy engineering has been implemented to quicken the Zn2+ diffusion in the solid phase and modulate the VO2 band gap.31–33 Nevertheless, there are only limited attempts to employ dual engineering of carbon and oxygen vacancy to enhance the electrochemical properties of VO2. Additionally, a straightforward and efficient method to simultaneously implement carbon and oxygen vacancy is urgently required.
Our study showcases a versatile and straightforward technique for producing carbon-coated VO2 nanobelts (VO2@C) with oxygen vacancies through C2H2 chemical vapor deposition. Structural and electrochemical analyses demonstrate that C2H2 heat treatment results in a carbon coating, oxygen vacancy, expanded lattice, and reduced grain size in VO2, thus enabling extra active sites, accelerating electron/ion transport, and preventing structural degradation. This leads to enhanced electrochemical performance compared to pure VO2 in AZIBs. The optimized VO2@C-350 composite electrode displays an impressive specific capacity of 391 mA h g−1 at 0.1 A g−1 over 100 cycles. It also maintains stability at 1 and 2 A g−1 throughout 2000 cycles and exhibits a reliable rate performance of 174 mA h g−1 at 5 A g−1. Our research proposes an innovative method for introducing carbon and oxygen vacancy to develop advanced cathode materials for AZIBs.
(1) |
Eqn (1) includes different variables such as σ, representing the Warburg factor, F for the Faraday constant, C for the zinc-ion concentration, A for the electrode surface area, T for the absolute temperature, n for the number of electrons per molecule, and R for the gas constant. To determine the value of σ, one can calculate the line slope using eqn (2).
Z′ = RD + RL + σω−1/2 | (2) |
We conducted galvanostatic intermittent titration technique (GITT) tests to determine the diffusion coefficient of Zn2+ in the electrode. As part of the GITT tests, participants were instructed to cycle for 20 minutes at 50 mA g−1 and rest for 2 hours after completing 10 activation cycles. During each relaxation period, the potential change indicated the overpotential of the corresponding discharge/charge state. To determine DZn2+, we employed Fick's second law and used a simplified equation.
(3) |
Eqn (3) includes various factors such as the mass of the electrode material (mB), its molar mass (MB), molar volume (VM), geometric area (S), potential equilibrium difference (ΔEs), change in cell voltage due to impulse current (ΔEτ), and average thickness of the electrode (L).
Fig. 1 (a) Scheme of the synthesis process for VO2@C nanobelts. SEM images for (b) VO2, (c) VO2@C-300, (d) VO2@C-350, and (e) VO2@C-400. (f) and (g) HRTEM images, and (h) EDS maps of VO2@C-350. |
The VO2-based samples’ crystal structures were analyzed using XRD. In Fig. 2(a), the XRD patterns of these samples are shown. It can be observed that all diffraction peaks correspond to VO2(B) (JCPDS no. 81-2392) having the space group of C2/m. Moreover, no noticeable impurities have been observed either before or after the C2H2 heat treatment. By analyzing the zoomed-in view of XRD patterns shown in Fig. 2(b), the diffraction peaks’ intensity decreases as the calcination temperature increases. This decrease in intensity suggests a reduction in crystallinity. Additionally, the characteristic peak (110) is observed to broaden and shift to a lower angle, indicating a decrease in grain size and an increase in interlayer spacing. These changes favor embedding and exfoliating zinc ions during discharging/charging. In Fig. S3 (ESI†), we can observe the Raman spectra of VO2-based samples. The peaks detected at 148, 288, 414, 530, and 997 cm−1 in VO2 indicate stretching and bending vibrations between the V–O within the layers.30,34 Additionally, the peak at 697 cm−1 shows the coordination of the vanadium atom with three oxygen atoms.22 Interestingly, the vibration patterns of VO2@C samples are comparable to those of the original VO2, suggesting that VO2's crystal structure remains intact after the C2H2 heat treatment. In addition, the presence of D and G bands in VO2@C samples confirms the formation of carbon.
Fig. 2 Structural characterizations of VO2-based samples. (a) and (b) XRD patterns, (c)–(e) high-resolution C 1s, V 2p, and O 1s XPS spectra, and (f) EPR spectra. |
An XPS analysis examined the samples’ electronic structure and surface composition. Based on the XPS survey spectra (shown in Fig. S4, ESI†), it can be determined that all VO2@C samples contain V, O, and C elements. The spectra of the VO2@C samples in Fig. 2(c) show three distinct peaks at 284.8, 286.2, and 288.4 eV in the C 1s region. These peaks indicate the presence of C–C, C–O, and CO bonds, respectively. These findings suggest that carbon has been successfully introduced.35,36 Pure VO2 exhibits two peaks at 515.8 and 522.8 eV in the V 2p spectrum, indicating the presence of V4+ in VO2, as depicted in Fig. 2(d).23 Following the C2H2 heat treatment, it was observed that the VO2@C samples displayed two additional peaks at 513.6 and 521.1 eV, which corresponded to V3+, indicating the formation of oxygen vacancies in VO2.32 The area ratios of V3+/V4+ calculated for VO2@C-300, VO2@C-350, and VO2@C-400 are 0.24, 0.27, and 0.29, respectively. These results indicate that the proportion of V3+ increases gradually with increasing calcination temperature, leading to an increase in the content of oxygen vacancies in the samples. The presence of these vacancies facilitates the rapid migration of ions and provides more channels for ion migration. From the O 1s spectra illustrated in Fig. 2(e), it can be inferred that the VO2@C samples contain oxygen vacancies. The peaks at 529.6, 531.1, 531.8, and 532.4 eV signify V–O, oxygen vacancy (Ov), C–O, and CO, respectively.32 Further evidence of the presence of oxygen vacancies was obtained through EPR spectroscopy, as shown in Fig. 2(f). The signal of VO2@C-350 exhibits a more pronounced symmetry peak at g = 2.0 compared to VO2. This is generally attributed to the presence of oxygen vacancy. TGA was utilized to determine the carbon mass fraction in the VO2@C composites produced at various temperatures, and the results are shown in Fig. S5 (ESI†). During heating in the air at a ramp rate of 10 °C per minute to 700 °C, there was a weight loss observed up to 200 °C. This was attributed to the loss of adsorbed water. C was converted to CO2 as the temperature increased, and VO2 was oxidized to V2O5.21,22 As a result, VO2@C-300, VO2@C-350, and VO2@C-400 have a carbon content of approximately 3.2, 5.1, and 16.5 wt%, respectively. These findings align with the carbon layer thickness observed on HRTEM.
We conducted a study to evaluate the Zn storage performance of VO2-based samples using a coin cell model (Fig. 3) to assess how oxygen vacancy and carbon coating affect the properties. In Fig. 3(a), the CV curves of VO2@C-350 are displayed at a scan rate of 0.2 mV s−1, ranging from 0.25 to 1.4 V. Based on our research, it appears that there is a notable redox coupling occurring at 0.37/0.56 and 0.92/1.05 V. This finding indicates a potential two-step zinc-ion (de)intercalation mechanism.20 Upon conducting the initial two scans, we observe stable redox couples, showing a remarkably reversible (de)intercalation reaction of Zn2+. The voltage curve for VO2@C-350's Zn storage process at 0.1 A g−1 is depicted in Fig. 3(b). In the initial cycle; the cell experiences an activation reaction that cannot be reversed. During the subsequent processes, two significant cathodic/anodic platforms occur at around 0.6/0.7 and 0.9/1.0 V, corresponding to the zinc ions’ (de)intercalation process. This is consistent with the findings derived from the analysis of the CV. In Fig. 3(c), the performance of VO2, VO2@C-300, VO2@C-350, and VO2@C-400 in terms of cycle performance and Coulombic efficiency (CE) at 0.1 A g−1 is demonstrated. Unfortunately, pure VO2 does not display good electrochemical activity, with an initial discharge capacity of only 319 mA h g−1. However, VO2@C-300 and VO2@C-350 show improved electrochemical activity with initial discharge capacities of 330 and 335 mA h g−1 after carbon cladding. Interestingly, VO2@C-400, with substantial carbon cladding, only delivers 260 mA h g−1 discharge capacity. Based on the VO2@C samples, there appears to be a gradual increase in the first few cycles, possibly attributed to the activation process of the electrodes. After 100 cycles, it has been observed that VO2@C-350 shows the highest electrochemical stability among the samples. It has a discharge capacity of around 391 mA h g−1 and no capacity decay. At the same time, the CE of C@VO2-350 is maintained at 99.5% throughout the cycles. After 100 cycles, pure VO2 has a capacity retention rate of 83.4%, with its capacity dropping to only 266 mA h g−1. In Fig. 3(d), we can see the rate performance of different samples at varying currents of 0.1 to 5 A g−1. Out of all the samples, VO2@C-350 has the most impressive rate performance. It can deliver discharge capacities of 331, 413, 406, 381, 350, and 174 mA h g−1 at 0.1, 0.2, 0.5, 1.0, 2.0, and 5.0 A g−1. It's important to note that the VO2@C-350's capacity remains consistent even when the rate drops abruptly to 0.1 A g−1. Fig. 3(e) displays the voltage curves for the discharge and charge of VO2@C-350. Furthermore, according to the data presented in Fig. 3(f), VO2@C-350 exhibits a higher rate performance compared to other cathodes that are based on VO2 for AZIBs, such as VO2−x(B),37 coin-shaped VO2,38 VO2 nanorods,39 β-VO2/CNTs,40 and VO2/Mxene.41 In Fig. 3(g), the performance of VO2@C-350 is observed throughout a lengthy cycling period, with its corresponding CE at 1 and 2 A g−1. Before the high-current test, the electrodes are activated with a slight current density of 0.1 A g−1. At a rate of 1 A g−1, the initial capacity is 438 mA h g−1, while at 2 A g−1, it is 342 mA h g−1. After undergoing 2000 cycles, the VO2@C-350 exhibits a discharge capacity of 350 and 254 mA h g−1 while maintaining 98.7% and 99.2% CE, respectively. These findings demonstrate the impressive cycling stability of VO2@C-350, indicating that the carbon cladding layer and oxygen vacancy can enhance conductivity and preserve the electrode material's structure.
Using EIS testing, it was discovered that VO2@C-350 had better reaction kinetics than the other materials. The Nyquist plots for these VO2-based samples exhibit comparable features (Fig. 4(a)). They all show a semi-circle that represents the charge transfer resistance (Rct) of the electrode/electrolyte interface, along with a straight line that denotes the Warburg impedance (Zw). According to Table S1 (ESI†), VO2@C-350 has a charge transfer resistance of only 92.2 Ω, which is lower than VO2 (119.1 Ω), VO2@C-300 (100.4 Ω), and VO2@C-400 (127.3 Ω). This suggests that VO2@C-350 has superior charge transfer kinetics. Fig. 4(b) illustrates a correlation between Z′ and ω−1/2 in the low-frequency range. The Warburg factor (σ), which represents the slope of the line, shows a direct correlation with DZn2+. After evaluating the Warburg factor, we were able to determine the diffusion coefficient of Zn2+ to be 9.7 × 10−11 cm2 s−1 for VO2, 1.7 × 10−10 cm2 s−1 for VO2@C-300, 2.7 × 10−9 cm2 s−1 for VO2@C-350, and 1.3 × 10−10 cm2 s−1 for VO2@C-400 (refer to Table S1, ESI†). We performed GITT measurements to evaluate DZn2+ in electrodes made from VO2. Fig. S6 (ESI†) displays the curves for voltage response and DZn2+ for VO2, VO2@C-300, VO2@C-350, and VO2@C-400, as well as their associated discharge/charge states. Based on the EIS analysis and GITT measurements, the order of DZn2+ in the electrodes appears as follows: VO2@C-350 > VO2@C-300 > VO2@C-400 > VO2. From the results, we can conclude that VO2@C-350 exhibits outstanding charge transfer and zinc-ion diffusion kinetics due to its optimized structure. Compared to the other samples, this contributes to its ability to achieve the highest storage capacity for Zn ions, cycling durability, and rate capability. We conducted CV tests on VO2@C-350 to determine the extent of diffusion-controlled and capacitance-controlled Zn ion storage. The results, displayed in Fig. 4(c), show that the CV curves of VO2@C-350 have similar shapes at 0.1–0.5 mV s−1. When the scan rate increases, the oxidation peak moves towards higher voltages, and the reduction peak moves towards lower voltages. The equation i = avb determines the peak current (i) based on the sweep frequency (v), with parameters a and b. When the value of b approaches 0.5, it suggests that ion diffusion processes are the primary factor influencing capacity. On the other hand, when b approaches 1, capacitive processes play a more significant role in determining capacity. By applying a logarithmic transformation to the current–sweep relationship shown in Fig. 4(d), the values of b for peaks 1, 2, 3, and 4 can be computed as 0.99, 0.86, 0.94, and 1.14, respectively. These values suggest that the pseudocapacitance contribution of VO2@C-350 is present throughout the redox process. An equation is used to determine the capacitance contribution: i = k1v + k2v1/2. The equation includes k1 and k2, which serve as percentage coefficients for the capacitance and diffusion factors in the overall capacity calculation. According to Fig. 4(e), the level of capacitance contribution rises considerably as the scan rate increases, resulting in advantageous outcomes for quick Zn2+ storage and cycle durability. According to the data shown in Fig. 4(f), when the scan rate is set at 0.5 mV s−1, the capacitance contribution reaches its peak at 66%. Moreover, we analyzed the Zn storage in the electrodes of VO2, VO2@C-300, and VO2@C-400 by employing the same analytical method. The results in Fig. S7–S9 (ESI†) indicate that the VO2@C-350 electrode exhibits a much higher capacitance contribution than the VO2 and VO2@C-300 electrodes. This highlights the superior performance of the VO2@C-350 electrode. Our research shows that the samples demonstrate a blend of ion storage mechanisms controlled by both capacitive and diffusion processes. Additionally, we observed that introducing oxygen vacancy and carbon coating into VO2 facilitated zinc-ion adsorption/desorption behavior.
We carried out ex situ XRD and XPS investigations to gain insights into the process of zinc-ion storage in VO2@C-350 (Fig. 5). In the first cycle, Fig. 5(a) displays ex situ XRD patterns of the VO2@C-350 electrode. The pristine electrode displays distinct diffraction peaks, including 25.3, 30.0, and 44.9°, which correspond to the crystal planes (110), (−401), and (−601) of VO2(B). Notably, the peaks observed during charging/discharging are consistently present, which suggests that the zinc-ion storage of VO2@C-350 is highly reversible and that the structural stability of the material is excellent. Moreover, new heights appear at 12.4 and 36.1° during discharge, which can be attributed to the Znx(OH)2V2O7·2H2O species.24,42 It seems that introducing zinc ions triggers a new phase, while their removal causes it to disappear. This implies that zinc storage relies on a co-intercalation/de-intercalation process of the Zn2+ and proton (H+). Fig. 5(b) displays the V 2p spectra of the VO2@C-350 electrode at different states. The ratio of V3+/V4+ in the pristine electrode is 0.24, which increases to 1.32 following discharge to 0.25 V due to H+/Zn2+ intercalation. Once charged to 1.4 V, the ratio of V3+/V4+ almost returns to its initial state. This indicates a reversible extraction of H+/Zn2+ from the VO2@C-350 structure. The Zn 2p spectrum (Fig. 5(c)) also supports this conclusion, as no Zn elemental is observed in the pristine electrode before charging and discharging. The Zn signal is significantly reduced during charging compared to the peaks during discharge, indicating that Zn2+ is extracted from VO2@C-350. However, trace Zn peak signals may be attributed to residual electrolytes on the electrode surface and irreversible Zn2+ intercalation in the VO2@C-350 electrode even after charging. Based on ex situ XRD and XPS analysis, it has been determined that VO2@C-350 exhibits an H+/Zn2+ storage process that follows a (de)intercalation reaction mechanism.
Fig. 5 Ex situ structural characterizations of VO2@C-350 electrode in the 1st cycle. (a) XRD patterns, (b) V 2p XPS spectra, and (c) Zn 2p XPS spectra. |
Footnote |
† Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d3ma00622k |
This journal is © The Royal Society of Chemistry 2023 |