Juan Carlos García-Mayorgaa,
Haret-Codratian Rosua,
Alma Berenice Jasso-Salcedob and
Vladimir Alonso Escobar-Barrios
*a
aAdvanced Materials Department, Instituto Potosino de Investigación Científica y Tecnológica A.C., Camino a la Presa San José, Lomas 4a Sección, San Luis Potosí, SLP 78216, Mexico. E-mail: vladimir.escobar@ipicyt.edu.mx
bDepartamento de Biociencias y Agrotecnología, Centro de Investigación en Química Aplicada, Blvd. Enrique Reyna Hermosillo No. 140, Saltillo, Coahuila 25294, Mexico
First published on 9th February 2023
The synthesis and characterization of polydopamine (PDA) using dopamine (DA) as the monomer and (hydroxymethyl)aminomethane (TRIS) as the oxidant is studied. The effect of temperature and TRIS concentration on the kinetics of dopamine polymerization is evaluated, and the kinetic parameters are also calculated. Three TRIS concentrations are used to assess their effect on DA polymerization kinetics. The reaction at 1.5 mmol of TRIS shows a sustained increase of the rate constant with temperature from 2.38 × 10−4 to 5.10 × 10−4 when the temperature is increased from 25 to 55 °C; however, not all reactions follow an Arrhenius law. In addition, the correlation between the synthesis parameters and morphological, structural, and thermal properties of polydopamine is established. The morphology of the PDA particles is evaluated by Scanning Electron Microscopy (SEM), the relationships between the diameter, distribution size, and the rate constant. Thermal characterization by Differential Scanning Calorimetry (DSC) shows an endothermic transition around 130 °C associated with the melting of PDA's regular structure. It is supported by structural studies, such as infrared and Raman spectroscopy and X-ray Diffraction (XRD), by observing a broad peak at 23.1° (2θ) that fits with a graphitic-like structure of PDA.
Additionally, thermodynamic and kinetic PDA synthesis studies are critical to establishing parameters like reaction order (n), pre-exponential factor (A), and activation energy (Ea). Such parameters are essential for polymerization control, affecting the material's final properties, and are critical to the technological use of the PDA. In this context, M. Salomäki et al.24 did a thermodynamic study of dopamine oxidation and cyclization dependence on pH and oxidants like transition-metal ions mainly focused on the early stages of the process. The authors proposed a general mechanism to understand the involved species during PDA polymerization and concluded that the most critical parameter for the process is the pK value. In the same way, the use of tuning radicals to control the size of PDA nanoparticles is reported by X. Wang et al.25 In the latter study, the authors concluded that the polymerization could be inhibited or terminated from the free radical scavengers, while the stable radicals catalyzed the formation of PDA seeds. A comparable study was carried out by M. Wu et al.26 who synthesized PDA through sodium hydroxide and developed a model about relationships between particle size, the molar ratio of DA, and oxidizing agent to control the particle diameter and distribution.
In addition, V. Ball et al.27 studied the film deposition kinetics influenced by pH, DA concentration, and their effect on thickness, morphology, roughness, and surface energy expressing the relationship between maximal thickness and kinetic constant to obtain thickness higher than 45 nm.
In summary, controlling the PDA polymerization reaction is essential since it determines its yield, particle size, and properties like photothermal effect, UV protection, and free radical scavenging activity.26,28 So far, the studies regarding the kinetics of PDA synthesis are few. One of the methods to have higher control over the synthesis of spheric PDA particles is the TRIS, which allows for obtaining small particles29 as well as the formation of films where TRIS lets to obtain maximal thickness in the deposition of PDA films;30 all of this in comparison with other buffers or alkalis like sodium hydroxide,31 sodium bicarbonate,32 ammonia,33 and phosphate solution.34 Nonetheless, relevant kinetics parameters like n, A, and Ea have not been provided regarding the synthesis of PDA spheres through TRIS. In this work, the aforementioned kinetic parameters are determined, and their relationship with the structure and properties of PDA is established.
The UV-vis spectrum of PDA suspension was carried out once it was washed and dried to remove any trace of DA. Afterward, the PDA was re-suspended in water with a water/PDA ratio of 20. Spectrum was measured in a range from 200 to 500 nm.
Regarding the color of the solution, from Fig. 1(C-1)–(C-3), it is clear that it changed according to the reaction extent and depending on its initial reaction temperature. A color change from pale yellow to dark brown indicates the self-oxidation of DA to obtain PDA.
The exact polymerization mechanism of PDA is still under debate, mainly due to its insolubility in all solvents. Nonetheless, there have been significant attempts to explain it. According to the literature,32,39 spontaneous auto-oxidation of dopamine accompanying intramolecular cyclization takes place, and alkali medium (pH ≥ 7.5) and dissolved oxygen are the key factors of the process.
Fig. 2A summarizes this process (illustration taken from ref. 40). Firstly, the catechol moiety of DA loses an e− and H+ to become dopamine semiquinone (DSQ), to oxidize again later, giving the dopamine quinone (DQ). Secondly, DQ undergoes intramolecular cyclization and oxidation to form leucodopaminechrome (LDC), which consequently gives rise to dopaminechrome (DC), which can re-arrange to DHI.
![]() | ||
Fig. 2 (A) Chemical route of the DA auto-oxidation,40 (B) PDA formation through the different oligomers.41 |
In addition, in analogy with the eumelanin, the hierarchical structure of PDA has been proposed, and three stages are established. The first stage is formed by oligomers of DA, DHI, or indolequinone (oxidized form of DHI, IDQ) species that could be covalently bounded by C–C in 2, 4, or 7 position for DHI and 2 or 5 position for DA, “covalent oxidative polymerization”; or they could be directly assembled by physical interactions (hydrogen bonds between oxidized species of catechol moieties), “physical self-assembly pathways”, as it is shown in Fig. 2B.
In contrast, other investigations have indicated that during the self-oxidation of DA, species like pyrrole carboxylic acids or catechol-containing carboxylates can be developed due to the oxidative destruction of the phenyl ring of the indole structures. These can be found as part of the structure of PDA, mainly when L-DOPA is used as a precursor.42 The second stage is built through stacking oligomers (trimers and tetramers) and non-covalent interactions like π–π interaction. In the last stage, aggregates are formed by weak non-covalent interactions between the structures.40,43 Additionally, temperature accelerates such oxidation, which is why a darker solution for the highest temperature (55 °C) is observed earlier than the reactions carried out at 25 and 40 °C (Fig. 1C). Thus, the influence of temperature on the reaction rate is evident, and an Arrhenius-type behavior is expected.
![]() | (1) |
![]() | (2) |
![]() | ||
Fig. 3 Change of dopamine concentration against time and exponential decline fitting for (A) 1.5 mmol TRIS, (B) 4.5 mmol TRIS, (C) 7.5 mmol TRIS, and (D) zoom of the reaction onset at 7.5 mmol TRIS. |
Applying natural logarithms to eqn (2), the mathematical equation corresponds to a linear equation (eqn (3)), where the slope corresponds to the reaction order n, and the intercept b corresponds to Ln(k), from which the rate constant can be obtained.
Ln(−r[DA]) = nLn([DA]) + Ln(k) | (3) |
Table 1 summarizes the values of the rate constant and reaction order from each temperature and TRIS concentration used.
T/°C | n1.5 | k1.5/min−1 | n4.5 | k4.5/min−1 | n7.5 | k7.5/min−1 |
---|---|---|---|---|---|---|
25 | 1.00 | 2.38 × 10−4 | 0.98 | 2.53 × 10−4 | 0.92 | 1.50 × 10−4 |
40 | 0.97 | 3.26 × 10−4 | 0.98 | 3.28 × 10−4 | 0.98 | 3.97 × 10−4 |
55 | 0.98 | 5.10 × 10−4 | 1.00 | 4.65 × 10−4 | 0.97 | 1.78 × 10−4 |
The synthesis of PDA with 1.5 mmol showed an increase in the reaction rate (Fig. 3A) as the temperature was increased, as was expected (Table 1). This behavior indicates that the reaction, under such conditions, follows typical behavior in terms of kinetics and the mechanism as proposed by Della Vecchia et al.29 Chemical kinetics—specifically the theory of collisions—indicates that when temperature increases in a chemical reaction, molecules' kinetic energy also increases. Consequently, the molecules have more energy to react and form products due to more collisions caused by the temperature increase,44 which exhibit an increment of 0.37 and 1.14 times when the temperature increase to 40 and 55 °C, respectively, concerning the rate constant at 25 °C.
The reaction order of the synthesis carried out with 1.5 mmol of TRIS was n ∼ 1 for every temperature. It means that the reaction of PDA formation depends linearly on the DA concentration. In other words, the reaction order of PDA synthesis implies the exponential decrease of DA concentration as a function of time, while the reaction rate decrease linearly as a function of concentration.
Fig. 3B displays the relationship of DA concentration vs. time at 25, 40, and 50 °C with 4.5 mmol of TRIS; the calculated values of the reaction order and rate constant for every reaction temperature were n ∼ 1 and k = 2.53 × 10−4, 3.28 × 10−4, and 4.65 × 10−4 min−1, respectively. In the same way, reactions carried out at 4.5 mmol TRIS show similar behavior concerning 1.5 mmol when the temperature increases; it represents an increment of the k as the temperature increase.
When the rate constants of 1.5 and 4.5 mmol TRIS are compared, a TRIS concentration effect can be noticed. TRIS molecule possesses three OH groups which are ionized when it is in solution; a higher concentration of OH− ions means that the Michael addition is accelerated.45 Michael's addition is an essential step in the DA auto-oxidation for the formation of DQ, where the catechol moiety of DA is oxidized, losing an e− and H+ with the participation of O2. However, this increase in the k value derived from hydroxyl ions concentration is limited to 25 and 40 °C since 55 °C is smaller than the k calculated with 1.5 mmol at the same temperature (Table 1).
As mentioned by M. Wu et al.,26 the synthesis of nanoparticles of PDA implies two stages. The first one is the formation of PDA seeds, which grow during the second stage. Variables like temperature, pH, oxidants, and concentration of DA during its polymerization affect both stages. Polymerization of DA is accelerated by a high initial concentration of OH− ions. In parallel to an increment in temperature, its effect leads to a higher nucleation rate of PDA particles and, thus, to forming more seeds.29,46 However, DA as a precursor for the PDA synthesis is consumed rapidly, and when more nuclei are formed, DA becomes unavailable for the particle growth stage. We assume that due to a slower growth stage of PDA particles, the observed k at 55 °C with 4.5 mmol TRIS could be lower than k with 1.5 mmol TRIS at the same temperature.
Fig. 3C and D illustrate the change in DA concentration over time for reactions with 7.5 mmol TRIS. Fig. 3D displays the change in DA concentration at 0, 1, and 2.5 minutes where a sudden decrease in DA concentration is observed as the TRIS solution was added. This reduction conveys an increment in TRIS concentration and temperature, which is correlated with the formation of seeds during the first stage of DA polymerization.
In order to estimate the oxidized DA and consumed for PDA nuclei, Fig. 4 shows the percent decrease in DA at the first instant after TRIS addition for all concentrations and temperatures. As is exhibited, for the reaction with 1.5 mmol TRIS, there is no sudden consumption of DA in the nuclei formation stage at the measurement's first time. However, for reactions at 4.5 mmol TRIS, one can notice a reduction of 2% in the DA concentration at 25 °C, which increases to 3.4% for the reaction at 55 °C; likewise, at 7.5 mmol TRIS, the DA concentration reduces by 11.7, 13.5, and 15.8% for 25, 40 and 55 °C, respectively. As mentioned before, OH− ions and temperature accelerate the DA oxidation, which promotes the formation of DQ, an essential step for the PDA seeds formation; from these results, it is also observed that an increment in TRIS concentration is more relevant for nuclei construction than an increment in temperature. At 25 °C, the consumption of DA was 0, 2.00, and 11.72% as the hydroxyl ions increased, an effect also observed for 40 and 55 °C, where the percentage of DA decrease was from 0 to 3.41 and 13.46%; and from 0.61 to 3.44 and 15.74%, respectively. In contrast to TRIS concentration, the lower effect of temperature could be explained as the dependence on dissolved oxygen, which is essential for the auto-oxidation of DA.47
![]() | ||
Fig. 4 Effect of the TRIS solution on DA consumption in the solution immediately after its addition (one minute after). |
From the results observed for DA polymerization with 7.5 mmol of TRIS was supposed that the reaction has two different rate constants. The first is associated with the sudden decrease of DA at the first moments of the reaction, and the second is related to the subsequent decrease of DA. Due to the high-speed consumption of DA, it was not possible to determine the rate constant at the first moments. At the same time, the reaction order was assumed to be a superior order, which explains the decrease in DA concentration over time.
From the profiles obtained with 7.5 mmol TRIS shown in Fig. 3C, the second rate constant, the reaction rate at 55 °C, is lower than that at 40 °C and is similar to that of 25 °C. The computing values for reaction order and rate constants at 25, 40, and 55 °C were n ∼ 1; and k = 1.50 × 10−4, 3.97 × 10−4, and 1.78 × 10−4 min−1, respectively. When the temperature rises to 40 °C, the rate constant increases 1.64 times in relationship with k at 25 °C, which corresponds with an Arrhenius behavior and an increment of OH− concentration.
Nevertheless, the rate constant decreases when the temperature increases to 55 °C. According to ref. 25, the use of free radical scavengers (i.e., edaravone) has an inhibition or termination effect during the DA polymerization, resulting in a decrement in particle size and yield. This effect occurs due to a reduction process promoted by edaravone during the oxidation of DA to DSQ species formation. It serves as an H-atoms donor to DSQ, which generates stable compounds. When the reaction is carried out at high temperatures, it implies the dissociation of water molecules, changing the concentration of H+ and OH− ions; in parallel, the generated species during DA oxidation with dissolved oxygen like H2O2 and HO2· (Salomäki, M. et al.24) also could be a source of H+. Herein, we assume that very high –OH ions concentrations (TRIS) affect the chemical kinetics of PDA polymerization, causing the inhibition/termination of the growth stage of PDA particles, which causes a lower k at 55 °C is obtained. In other words, when rate constants at 55 °C at different TRIS concentrations (Table 1) are compared, it is observed that reversibility in the DQ formation and inhibition/termination effects are more substantial when temperature and TRIS concentration increased, affecting the rate constant. Similar results were reported by X. Wang et al. where higher pH values (>9.55) gave lower yields.
According to chemical kinetics principles, most chemical rate constants increase as the temperature increases, and the Arrhenius equation (eqn (4)) expresses this relationship.
![]() | (4) |
The Arrhenius parameters, activation energy (Ea), and pre-exponential factor (A) were calculated from the plot of Ln(k) against 1/T that gives a straight line (y = mx + b) where the slope (m) is m = −Ea/R, while b = Ln(A) provides the pre-exponential factor, see Table 2. The Ea is the minimum kinetic energy that reactants must have to generate products. Thus, 20.6 kJ mol−1 is the Ea computed for the reaction at 1.5 mmol while, for 4.5 mmol, it decreases to 16.48 kJ mol−1. This effect means that a high pH (concentration of OH−) reduces the activation energy—four-fifths compared to 1.5 mmol—needed to carry out the reaction of DA polymerization. In addition, the calculated Ea at 7.5 mmol TRIS, just for 25 and 40 °C, is 50.27 kJ mol−1. High activation energy values imply a strong dependence of the rate constant on temperature, a result supported by the above-calculated rate constants. Moreover, in the case of 40 and 55 °C, the obtained Ea = −45.5 kJ mol−1 describes the rate decrease as the temperature increases.
1.5 mmol | 4.5 mmol | 7.5 mmol | |
---|---|---|---|
Ea/kJ mol−1 | 20.60 | 16.48 | 50.27 |
A/min−1 | 0.94 | 0.19 | 96![]() |
Fig. 5 shows the plot Ea vs. Ln(A); as is observed, A for DA polymerization increases linearly with Ea. This relationship is explained by Brønsted acid sites (or active sites) in catalysts.48,49 According to these works, an increase in active centers corresponds to a higher value of A; also, due to statistical and thermodynamic reasons, these active sites should be more numerous with decreasing energy. Additionally, they are less effective with lower energy. In other words, low energy in the active centers is accompanied by a high value of Ea.
Above all, this linear relationship between Ea and Ln(A) could be explained by DA polymerization in the growth stage. DA monomers react on the surface of previously formed PDA particles, where active sites like catechol moiety (acid site) and secondary amine (basic site) can affect the auto-oxidation and polymerization of DA.
Material | Diameter/nm | SD | |
---|---|---|---|
1.5 mmol | 25 °C | — | — |
40 °C | 438.4 | 255.6 | |
55 °C | 358.8 | 181.7 | |
4.5 mmol | 25 °C | 661.2 | 148.0 |
40 °C | 424.6 | 40.9 | |
55 °C | 173.3 | 11.3 | |
7.5 mmol | 25 °C | 564.6 | 29.1 |
40 °C | 276.4 | 18.6 | |
55 °C | 334.3 | 16.9 |
The Ostwald ripening process explains a wide distribution of diameter particles at 40 and 55 °C.50 This process occurs when little particles are dissolved; the DA monomers from the surface of the smaller particles migrate to larger ones, resulting in bigger particles and wide distribution due to the higher surface energy of smaller particles; according to the Gibbs–Thompson relationship, these tend to dissolve.
The micrographs at 4.5 mmol TRIS (Fig. 6D–F for 25, 40, and 55 °C, respectively) show well-defined spherical particles with a narrow distribution (Table 3). A more spherical morphology is observed as a result of a higher concentration of TRIS than reactions at 1.5 mmol TRIS. Additionally, the temperature also affects the size distribution and average diameter.
Results from 7.5 mmol TRIS concentration at various temperatures (Fig. 6G–I) also show well-defined particles with average diameters of 564.6, 276.4, and 334.3 nm and SD of 29.1, 18.6, and 16.9 nm, respectively. In the same way, the effect of higher TRIS concentration gives better-defined particles. However, the diameter of PDA particles is not correlated with temperature since an increment from 25 to 40 °C represents a decrement from 564.6 to 276.4 nm; but when the temperature increases to 55 °C, the average size increases to 334 nm. In order to explain the change in particle size, the rate constant has a better fit. Although the temperature affects the rate constant, the inhibition/termination effect on PDA polymerization affects the rate constant and particle size, as mentioned before. In summary, the polymerization of PDA strongly depends on TRIS concentration and temperature; higher concentrations of TRIS encourage well-defined spherical particles and affect the particle size and distribution, an equally promoted effect by temperature from the rate constant.
![]() | ||
Fig. 7 Thermogravimetric analysis of (A) dopamine hydrochloride (DA·HCl) and (B) synthesized PDA at 25 °C. |
In the case of PDA, Fig. 7B shows the TGA thermograms of PDA synthesized with 1.5, 4.5, and 7.5 mmol TRIS. All the materials show similar and multistep weight loss associated with chemical heterogeneity. Four steps in the thermal degradation of PDA are identified; the first one is related to the evaporation of weakly bound water due to high PDA hygroscopicity,52 observed from 25 to 100 °C. The second one—between 100 and 240 °C—corresponds to the release of intramolecular, strongly-bonded water.53 The third step associated with the decomposition of aliphatic components52 presented in PDA originated from DA molecules non-oxidized during the polymerization. Finally, with a final average mass retention of 56.2%, the last step from 420 to 700 °C matches with aromatic compounds like catechol or the o-benzoquinone moieties that decompose in this temperature range.54
Table 4 summarizes the loss in weight of PDA computed for each material at the final temperature of the four-step degradation process. The weight loss at 100 °C oscillates between 6.30 and 7.12%, with differences of 0.31%; this was the highest difference value of the four steps losses associated with the high material hygroscopicity. Molecular water trapped between PDA microstructure from the synthesis medium needs more heat to be released; the average weight loss of this process was 5.57%, with narrow differences (variation of 0.17%). The average weight loss of 25.8% at 420 °C is 0.19%, similar to the variation at 700 °C (0.13%). Low differences and similar behavior of PDAs after 240 °C could be associated with the similar chemical composition of PDA synthesized under different conditions.
Material | Weight loss/% | DSC results | |||||
---|---|---|---|---|---|---|---|
25–100 °C | 100–240 °C | 240–420 °C | 420–700 °C | Melting peak/°C | Enthalpy/J g−1 | ||
1.5 mmol | 25 °C | 6.42 | 12.13 | 26.04 | 43.92 | 125.0 | 304.5 |
40 °C | 6.82 | 12.34 | 25.60 | 43.66 | 124.5 | 340.9 | |
55 °C | 6.39 | 12.00 | 25.79 | 43.93 | 137.2 | 346.6 | |
4.5 mmol | 25 °C | 6.30 | 12.05 | 26.03 | 43.89 | 98.1 | 308.2 |
40 °C | 7.12 | 12.39 | 25.82 | 43.89 | 99.1 | 412.5 | |
55 °C | 6.97 | 12.44 | 25.62 | 43.67 | 100.8 | 297.9 | |
7.5 mmol | 25 °C | 6.42 | 12.13 | 26.04 | 43.92 | 139.2 | 307.5 |
40 °C | 6.39 | 12.00 | 25.79 | 43.93 | 123.9 | 338.9 | |
55 °C | 6.82 | 12.34 | 25.60 | 43.66 | 145.7 | 280.2 |
The literature about natural and synthetic melanin postulates that these materials do not have a defined structure, considering them amorphous materials.54–57 On the other hand, E. Coy et al.58 have reported contradictory results for synthesized PDA characterized by Raman spectroscopy without any thermal treatment, which shows characteristics related to carbonized PDA particles; this material displays regular zones that indicate nanocrystalline graphite-like structure.59 In addition, according to polymers science,60,61 characteristic endothermic peaks observed by DSC are associated with the fusion of crystalline regions present in the microstructure of polymers.62 The crystalline fraction can be computed by the quotient of the melting enthalpy (heat associated with the fusion process) measured and the melting enthalpy of the completely crystalline material.
The first authors that propose the relationship between the endothermic process of natural and synthetic melanin and a phase transition based on the granule nucleus organization were Simonovic B. et al.63 The DSC thermograms of PDA are shown in Fig. 8. A broad endothermic peak with a maximum is observed between 98 and 146 °C; this first-order transition is linked with the melting process of PDA. As mentioned above, the chemical composition of PDA consists of layers (oligomers) composed of 3–4 units of mainly 5,6-dihydroxindole and DA molecules covalently bonded. Simultaneously, these layers interact by π–π systems, giving rise to ordered short-range regions. These arrangements, known in polymer science as lamellae crystals, suggest the presence of crystalline regions in PDA, which are destroyed by heating, explaining the transition observed by DSC.
![]() | ||
Fig. 8 Thermograms obtained from PDA synthesized at (A) 1.5 mmol, (B) 4.5 mmol, and (C) 7.5 mmol for each temperature. |
Thermograms show the effect of synthesis conditions through the form—narrow or broad—of the endothermal peak (melting temperature) and melting enthalpy. Such thermograms indicate different melting temperatures due to crystallite imperfections and non-uniformity in their size. For instance, Yu, X. et al.64 reported dark domains of graphite-like nanostructures with short-range (2–3 layers) and large-range (∼40 layers) on calcinated PDA particles using High-Resolution Transmission Microscopy.
Fig. 8 illustrates the PDA thermograms synthesized with 1.5, 4.5, and 7.5 mmol TRIS at the three temperatures. Thermograms from synthesis at 4.5 mmol TRIS (Fig. 8B) show similar melting enthalpies compared with 1.5 and 7.5 mmol TRIS, but the melting points are lower (between 27 and 35 °C, Table 4). These results indicate that pH (TRIS concentration) and temperature have an essential effect on the conformation of PDA microstructure with an accentuated effect at 4.5 mmol TRIS concentration.
The associated enthalpy for each material is also listed in Table 4. It is worth mentioning that there are no data in the literature about melting enthalpy for crystalline PDA. Thus, it is not possible to calculate the crystalline fraction for these materials. However, if it is assumed that the PDA with the higher enthalpy value has the highest crystalline fraction (100%), which was obtained with 4.5 mmol TRIS at 40 °C, then 7.5 mmol TRIS at 55 °C produces the PDA with the lower crystalline fraction, 67.98%.
On the other hand, a minimum effect of TRIS concentration on the melting enthalpies for 1.5, 4.5, and 7.5 mmol at 25 °C is noticed. When the temperature increases to 40 and 55 °C, the effect of TRIS concentration is substantial; for instance, at 1.5 mmol, the temperature favors the formation of crystalline fractions in PDA, while the crystalline fractions at 40 °C are higher than those at 25 °C, at 4.5 and 7.5 mmol. But at such TRIS concentration and 55 °C, the crystalline fraction is reduced regarding that at lower temperatures. It is assumed that this effect relates to the chemical kinetics of PDA synthesis; at low TRIS concentration, the effect of temperature is directly proportional to the crystalline fraction.
On the contrary, this relationship changes when TRIS concentration increases to 7.5 mmol, which modifies the rate constant, see Fig. 9A. According to Yu, X. et al., there are more stacking layers on the shell than in the inner of PDA particles, which could be affected by the inhibition/termination or Ostwald ripening process on the surface of particles during the growth stage.
![]() | ||
Fig. 9 Relationship between (A) rate constant and enthalpy of fusion, and (B) synthesis and melting temperature. |
A correlation between the endothermal transition and inner water molecules in the microstructure also can be established in the 100–240 °C range, where the melting of crystalline regions of PDA led to water molecules–from reaction media—to be released. Nonetheless, the enthalpy associated with this process is much lower than the associated melting enthalpy.53,63
Fig. 9B illustrates the correlation between the synthesis and melting temperature, where most crystalline regions disappear; this also depends on crystallite defects or size. Results for 4.5 mmol TRIS show a minimum effect of the temperature on melting point; that means greater homogeneity of the crystalline regions or a reduced number of crystal defects. When the polymer is heated, the chains begin to move gradually as temperature increases and the crystalline domains are fused. The movement of chains depends on many aspects like mainchain symmetry and flexibility, polarity, tacticity, type/size of side-groups, and residual monomer/solvent.65 As mentioned above, PDA is constituted by oligomers, which are made up of 2–8 monomers,64,66 such as DHI and DA, in the beginning.
It is relevant due to the rigidity of the DHI compared to DA molecules; DHI has two aromatic rings, which reduce the flexibility, while the DA has a catechol moiety and an aliphatic branch which make its movement less restrictive. In the same way, oligomers with more monomers (e.g., 8 DHI molecules) mean a more restricted motion than smaller oligomers (e.g., 4 DHI). Results at 1.5 and 7.5 mmol show a considerable difference in melting temperatures, but with similar tendencies; this is ascribed to different ratios of DHI/DA monomers and polymerized degree of oligomers (2–8 units) derived from synthesis conditions.
Table 5 lists the ratio between primary and secondary amine intensities.70 A ratio below unity is observed for all materials; it specifies a higher quantity of secondary amine groups, indicating a conformation based mainly on DHI monomers. The 4.5 mmol TRIS concentration displays a high ratio of 1075/1150 cm−1. A more subtle difference is observed in the 1600/1525 cm−1 ratio; it could be due to the overlapping bands from the benzene ring (CC, 1560–1630 cm−1) and amine groups. These results—in comparison with the other two concentrations—demonstrate a higher presence of DA monomers in PDA, which supports the DSC results where the aliphatic branch, that even having a 3-dimensional structure since it is aliphatic the primary bonds allows rotational movement, which needs less energy to begin to move compared to the aromatic structure of DHI, which is more voluminous and rigid.71,72
Material | Intensity ratio (NH2/NH) | ||
---|---|---|---|
1600/1525 cm−1 | 1075/1150 cm−1 | ||
1.5 mmol | 25 °C | 0.72 | 0.24 |
40 °C | 0.91 | 0.18 | |
55 °C | 0.92 | 0.23 | |
4.5 mmol | 25 °C | 0.85 | 0.31 |
40 °C | 0.87 | 0.32 | |
55 °C | 0.86 | 0.30 | |
7.5 mmol | 25 °C | 0.74 | 0.20 |
40 °C | 0.84 | 0.20 | |
55 °C | 0.79 | 0.24 |
On the other hand, the higher presence of secondary amine in materials obtained at 1.5 and 7.5 mmol TRIS is associated with favoring DA cyclization (DHI monomers) and contributes to a more rigid structure observed through the differences and higher values of melting temperatures—DSC results.
In addition, Fig. 11 displays the Raman spectra of synthesized PDA; two distinct bands, D (amorphous band—sp3 and H) and G (graphitic band—sp2), are shown in all samples. The first one, the D-band at ∼1374 cm−1, and the second one, the G-band at ∼1579 cm−1, originated from linear stretching of C–C bonds inside the rings and in-plane stretching of the aromatic rings,59,73 respectively. The intensity ratio (ID/IG) is utilized to identify the degree of defects in a material where a low ratio indicates a low number of defects; consequently, the material presents a more graphitic structure with an sp2 phase. The ID/IG ratio for 1.5 and 7.5 mmol TRIS displays similar values. These were below the unity that signifies the predominance of the graphite-like structure (sp2 bonds) associated with the π–π stacking layers model as has been proposed for PDA; on the other hand, higher values of ID/IG ratio at 4.5 mmol reveal a lower graphite-like arrangement.
Notwithstanding, a specific analysis of the position of the G-band indicates a gradual blue shift (Fig. 12). According to Li, H. et al.,57 the change of the G-band (to blue) is associated with carbonized PDA, where the amorphous carbon structure of PDA is converted to nanocrystalline graphite. The PDA synthesized here was not carbonized, but a relationship was established between the synthesis temperature and the blue shift, Fig. 12. We think that the synthesis temperature can also affect the PDA structure.
In particular, the low positions of the G-bands and the high ID/IG ratio for materials obtained at 4.5 mmol TRIS concentration compared with the other two concentrations could be explained due to the presence of DA monomers. Monomers constituted by DHI molecules are planar structures with π–π bonds (sp2 hybridization), allowing monomers to stack in a graphitic-like structure. Nevertheless, when DA molecules form part of oligomers, the presence of π–π bonds is reduced, and sp3 hybridization (characteristic hybridization of amorphous carbon material) increases.74
The center peak of PDA spectra for all materials was located at 23.1 ± 0.1 (2θ), which indicates a typical graphitic-like structure and suggests a d-spacing of ∼3.4 Å. No effect from the synthesis conditions is observed for the XRD spectra; it can be associated with the reaction media since the water was used as the solvent.
Fig. 14 shows the two most used monomers to explain the PDA structure and its stacking as a graphitic-like structure. Fig. 14A presents an oligomer formed by four DHI molecules and its different oxidized forms; this cyclic model (Cyclotetramer) proposed by Meng and Karixas has been obtained through density functional theory (DFT) calculus, and despite explaining the optical absorption of natural melanin and PDA, it has not been experimentally proven.76 On the other hand, Fig. 14B illustrates the PDA monomer structure based on spectroscopic and DFT results, the Liebscher model.77 In this model, the composition of oligomers is formed by a mixture of DHI units with different unsaturation degrees (DHI and its oxidized forms) and open-chain dopamine units (DA) united covalently by carbon atoms in the 4 and 7 positions; results that support the presence of PDA chains of this kind also were reported by P. Delparastan et al.,78 where also was identified the interaction between chains by reversible non-covalent interactions.
According to the results obtained from the thermal and spectroscopic analysis, the presence of DA units in the PDA chains has been inferred; consequently, the Liebscher model adjusts and describes the observed properties of the PDA. Finally, Fig. 14C shows the stacking structure of PDA chains with a d-spacing of ∼3.4 Å supported by the π–π interactions.
The correlation between PDA morphology and TRIS concentration/temperature is well established in the literature. Nonetheless, this work has proven that morphology is mainly related to the rate constant, which depends on TRIS concentration and temperature but does not behave linearly concerning these conditions.
It has been identified that the ratio of primary and secondary amines in the PDA is essential to understanding its structure since the presence of primary amines—associated with DA monomers—affects it, as DSC thermograms and FT-IR spectra showed.
In this work, the existence of crystalline regions, within the PDA particles, was corroborated by DSC, Raman, and XRD analysis in contraposition to conventionally reported amorphous structure.
This journal is © The Royal Society of Chemistry 2023 |