Youngseul Choa,
Kyu Sang Leeb,
Shuqing Piaob,
Taek-Gyoung Kimc,
Seong-Kyun Kangc,
Sang Yoon Parkd,
Kwanghyun Yoo*c and
Yuanzhe Piao*abd
aProgram in Nano Science and Technology, Graduate School of Convergence Science and Technology, Seoul National University, 145 Gwanggyo-ro, Yeongtong-gu, Suwon-Si, Gyeonggi-do 16229, Republic of Korea. E-mail: parkat9@snu.ac.kr
bDepartment of Applied Bioengineering, Graduate School of Convergence Science and Technology, Seoul National University, 145 Gwanggyo-ro, Yeongtong-gu, Suwon-Si, Gyeonggi-do 16229, Republic of Korea
cBETTERIAL Co., 307, 52, Sagimakgol-ro, Jungwon-gu, Seongnam-si, Gyeonggi-do, Republic of Korea. E-mail: kyoo@betterial.io
dAdvanced Institutes of Convergence Technology, 145 Gwanggyo-ro, Yeongtong-gu, Suwon-si, Gyeonggi-do 16229, Republic of Korea
First published on 3rd February 2023
Silicon microparticles (SiMPs) show considerable promise as an anode material in high-performance lithium-ion batteries (LIBs) because of their low-cost starting material and high capacity. The failure issues associated with the intrinsically low conductivity and significant volume expansion of Si have largely been resolved by designing silicon/carbon composites using carbon nanotubes (CNTs). The CNTs are important in terms of stress dissipation and the conductive network in Si/CNT composites. Here, we synthesized a SiMP/2D CNT sheet wrapping composite (SiMP/CNT wrapping) via a facile freeze-drying method with the use of highly dispersed single-walled CNTs. In this work, the well-dispersed CNTs are easily mixed with Si, resulting in effective CNT wrapping on the SiMP surface. During freeze-drying, the CNTs are self-assembled into a segregated 2D CNT sheet morphology via van der Waals interactions. The resulting CNT wrapping shows a unique wide range of conductive networks and mesh-like CNT sheets with void spaces. The SiMP/CNT wrapping 9:1 electrode exhibits good rate and cycle performance. The first charge/discharge capacity of SiMP/CNT wrapping 9:1 is 3160.7 mA h g−1/3469.1 mA h g−1 at 0.1 A g−1 with superior initial coulombic efficiency of 91.11%. After cycling, the SiMP/CNT wrapping electrode shows good structural integrity with preserved electrical conductivity. The superior electrochemical performance of the SiMP/CNT wrapping composite can be explained by an extensive conductive CNT network on the SiMPs and facile lithium-ion diffusion via mesh-like CNT wrapping.
The preparation of silicon-based composites combined with carbonaceous materials imparts valuable properties to Si, whereby the challenges of huge volume expansion and poor electronic conductivity can be simultaneously resolved.3,6,8,9 Among the various carbon materials, carbon nanotubes (CNTs) have received extensive consideration in the targeting of efficient composite design.10–13 From a structural viewpoint, the superb mechanical stabilities and excellent electrical conductivities of CNTs have been reported to overcome the aforementioned intrinsic issues of Si electrodes.14–16 Despite the impressive advances, Si/CNT composite design typically requires complicated procedures.17–19 Furthermore, the intrinsic properties of CNT, such as severe entanglement and agglomeration owing to π–π interactions and van der Waals forces, are recognized as critical drawbacks.13,14 The CNT distribution is an important factor to dissipate Si volume changes and generate a well-dispersed conductive network. Recently, CNT dispersions have been introduced as a conductive additive in a wide range of micron-scale active material particles, including silicon microparticles (SiMPs).14 The resulting segregated CNT network in the electrode could improve both the mechanical properties and electrical conductivity with low charge-transfer resistance. For this reason, it is highly desirable to further develop a Si/CNT composite by taking advantage of its structural properties. According to previous studies, the carbon wrapping structure of Si/C composites was also found to effectively mitigate volume changes of Si and promote extensive conductive networks.9,20
For this reason, herein, we prepared a SiMP/2D CNT sheet wrapping composite (SiMP/CNT wrapping) via freeze-drying by using highly dispersed single-walled CNTs. Lyophilization is one of the widely used methods for composite preparation in energy storage systems.21–23 During freeze-drying, the well-dispersed CNT networks are simply self-assembled into segregated CNT sheets, resulting in efficient wrapping on SiMPs. In particular, the CNT dispersion formed a unique CNT sheet morphology without agglomeration of the CNTs. In addition, the well-dispersed CNTs are easily mixed with the SiMPs in the preparation step. The optimized structural properties of the SiMP/CNT wrapping composite were investigated by controlling the weight ratios between SiMP and CNT. The thickness of the CNT wrapping sheet can be varied with the amount of CNT dispersion. The resulting SiMP/CNT wrapping composite was tested as an anode material in lithium-ion batteries. The optimized SiMP/CNT wrapping 9:1 composite exhibits superior rate and cycling performance with high capacities. In addition, the SiMP/CNT wrapping 9:1 electrode shows high initial and later-cycle coulombic efficiencies, implying stable SEI formation and the structural integrity of the composite. The as-synthesized SiMP/CNT wrapping composite has multiple attractive advantages. The tight CNT wrapping on the SiMPs could alleviate the volume expansion of Si and preserve electrical conductivity during repeated charge and discharge cycles. Furthermore, the mesh-like CNT sheets composed of 1D CNTs are expected to offer a wide range of extensive conductive networks and facile lithium-ion diffusivity, which endow SiMP with electrochemical activity upon cycling. This work provides useful guidelines for SiMP/CNT composite design using well-dispersed CNTs and suggests the easy preparation of a segregated 2D CNT wrapping network via lyophilization.
Based on the unique CNT architecture in Fig. 1b–d, we further explored the well-dispersed CNTs and the effect of the preparation method on the structural properties of the CNTs. Fig. 2a shows SEM images of pristine SWCNT powder without any purification or chemical treatment. The severe CNT aggregation and strongly entangled CNTs in Fig. 2a could be due to intrinsic properties of the SWCNTs, such as van der Waals forces and strong π–π interactions.26,27 The intrinsically strong aggregation of SWCNTs limits their application and usage in a wide range of research areas.28,29 As shown in Fig. 2b and c, the SEM and transmission electron microscopy (TEM) images of the CNT dispersion display well-dispersed SWCNT networks without CNT bundle aggregates. For the SEM analysis, the CNT dispersion was dropped on a Cu foil and dried in a vacuum oven, which is the same as the electrode preparation in the experimental section. Furthermore, the dispersibility of the CNT dispersion was investigated, as shown in Fig. S2†. In Fig. S2a and b†, the digital photographs of the CNTs show highly dispersed SWCNTs. The uniform dispersion was easily observed with the naked eye. When it was applied to slide glass, the even coating of the SWCNT dispersion without aggregates indicated its superior dispersibility (Fig. S2c†). The dispersion stability of the CNT dispersion continued even after 24 hours (Fig. S2d and e†). Optical microscopy (OM) images of well-dispersed SWCNTs and pristine SWCNTs are shown in Fig. S2f and g†. Compared to the severely entangled CNT aggregates of the pristine SWCNT, the SWCNT dispersion exhibits good dispersion properties. Our approach to the preparation of the SiMP/CNT wrapping composites involved lyophilization of a mixed solution of SiMPs and the SWCNT dispersion. To determine the necessary experimental conditions to obtain the unique CNT architecture, we prepared CNT samples using an oven-drying or freeze-drying method. Detailed information about the preparation of the oven-dried and freeze-dried CNT samples is provided in the experimental section. As shown in Fig. 2d, the digital photograph of the oven-dried CNTs shows a dense CNT film. Accordingly, thick and closely packed CNT networks were observed in the SEM images of the oven-dried CNT sample (Fig. 2e). In contrast, the freeze-dried CNT dispersion sample exhibited different structural properties. The freeze-dried CNTs in Fig. 2f are similar to an aerogel structure. The 2D CNT structure composed of SWCNTs is shown in the SEM images of the freeze-dried CNT sample in Fig. 2g. From the structural view of the freeze-dried CNT sample, each CNT sheet was created in parallel to each other, indicating that self-assembly occurred during freeze-drying.24,25 In addition, we consider that the segregated CNT network would be a result of the van der Waals interactions between CNTs.12,14 Therefore, we speculate that the formation of thin 2D CNT sheets is provided by the chemical interaction between CNTs and the freeze-drying method. However, the segregated 2D CNT network was not formed when we freeze-dried aqueous pristine SWCNT powder dispersion due to severe aggregation between SWCNTs (Fig. 2h and i).
Hereafter, the SiMP/CNT wrapping 8:2 and SiMP/CNT wrapping 9:1 composite are denoted as 8:2 and 9:1 in figures and data. Fig. 3a and b shows SEM images of counterparts for SiMP/CNT wrapping composites such as SiMP and SWCNT sheets. The SEM image in Fig. 3a displays the irregular shape of pristine Si microparticles with a size range of around 1–5 microns. In Fig. 3b, extensive 2D CNT sheets were observed in the SEM image. Based on the unique CNT architecture in Fig. 1b–d, we prepared SiMP/CNT wrapping composites following the same synthetic route as for 2D SWCNT sheet fabrication. In Fig. 3c, the digital photograph of the freeze-dried SiMP/CNT wrapping 8:2 composite shows a dense aerogel structure. In an attempt to investigate the morphological and structural properties, we prepared SiMP/CNT wrapping composites with different weight ratios between the SiMPs and SWCNT dispersion. As shown in Fig. 3d and e, all the obtained SiMP/CNT wrapping composites with different weight ratios between SiMPs and CNTs show a unique 2D CNT sheet wrapping structure that is similar to that of the 2D CNT sheets (Fig. 3b). The result implies that the 2D SWCNT sheets are formed via freeze-drying even in the presence of SiMPs. Overall, the SiMPs are wrapped with a wide range of 2D CNT sheets, which were segregated and van der Waals-bonded SWCNT networks. High-magnification SEM images of SiMP/CNT wrapping 8:2 shows that the SiMP particles are effectively wrapped by a 2D CNT membrane (Fig. 3d). Even with a smaller SWCNT dispersion content, the resulting SiMP/CNT wrapping 9:1 composite also shows a similar CNT network but thin CNT sheet coverage on the SiMPs (Fig. 3e). The less-dense CNT sheet wrapping of the SiMP/CNT wrapping 9:1 composite could be due to the lower amount of SWCNT dispersion. With increased content of SWCNT dispersion, the resulting SiMP/CNT wrapping 8:2 sample maintained the extensive CNT wrapping network; however, thicker 2D CNT sheets were formed. This demonstrates that the changes in the content of the components could affect the resulting structure of the SiMP/CNT wrapping composite.30 Since the 2D CNT sheets effectively wrapped the SiMPs, we further estimated that the 2D SWCNT sheets, which consist of mechanically strong SWCNTs, could act as an efficient buffer matrix inside the composite for preserving its structural integrity against the huge volume changes of Si.14 Fig. 3f shows a digital photograph of an aqueous mixture of SiMPs and CNTs. Compared to the pristine SWCNTs, the CNT dispersion + SiMP mixture exhibits good dispersion without severe aggregation of the CNTs. The well-mixed CNT dispersion + SiMP could ensure CNT distribution in the composite, resulting in effective Si volume change dissipation and an evenly dispersed conductive network. As shown in Fig. 3f, a digital photograph of the freeze-dried SiMP/pristine SWCNT composite shows a powder-type sample. To investigate the distribution of SiMP and CNT in the composite, we conducted SEM analysis with energy-dispersive X-ray spectroscopy (EDS) mapping. Compared to the aggregated CNT networks in the SiMP/pristine SWCNT composite, the SiMP/CNT wrapping 9:1 composite shows extensive 2D CNT wrapping on the SiMPs (Fig. 3g and h). To further investigate the morphological features of the self-assembled 2D CNT wrapping network formation, the effect of the silicon particle size and weight ratio between silicon and the CNT dispersion on the Si/CNT composite were tested, as shown in Fig. 3i, S3 and S4†. Therefore, we also prepared a Si/CNT composite using silicon nanoparticles with a diameter of 50 nm with different weight ratios between the SiNP powder and SWNCT dispersion. According to previous studies, there was a prerequisite that the particles should be micron-sized to form a segregated CNT network.12,14 However, the effective hierarchical CNT network was simply formed when we freeze-dried well-dispersed CNTs (Fig. 3b). For the micron-scale Si, 2D CNT wrapping is formed on the SiMPs, and the CNT wrapping thickness can be varied by controlling the CNT content. Compared to the SiMP/CNT sample (Fig. 3c), the digital photograph of the freeze-dried SiNP/CNT composite exhibits a loosely interconnected aerogel structure, which might be due to the larger surface area of the silicon nanoparticles. Although the SiNP/CNT 9:1 composite shows a non-segregated structure (Fig. S3†), an increased amount of CNTs results in the formation of embedded SiNPs in a micro-scroll CNT structure via freeze-drying (Fig. 3i and S4†).10 During the freeze-drying, the well-dispersed CNT could form a 2D assembly even with nanosized silicon particles. This result provides a guideline to develop segregated 2D CNT network-based Si composites by selecting different sizes of silicon particles or adjusting the proportion between Si and well-dispersed SWCNTs.
To characterize their structural properties, detailed analyses were conducted of the SiMP, SWCNT dispersion, and SiMP/CNT wrapping composites. Due to the liquid-type property of the SWCNT dispersion, the SWCNT dispersion was freeze-dried for material characterization. As shown in Fig. 4a, the sharp peak in the Raman spectrum of SiMP at around 500 cm-1 corresponds to crystalline Si.4,31 In addition, the SWCNTs show a Raman spectrum with distinctive peaks. The peaks at the low wavenumber side at around 1350 cm−1 and at around 1590 cm−1 are derived from the radial breathing mode (RBM), defect, and in-plane vibration of a six-membered ring of carbon materials, respectively.32 According to previous research, SWCNTs shows splitting of the G band into G+ and G−, which are referred to as the longitudinal wave mode and transverse wave mode perpendicular to the axis.33 In Fig. 4a, the Raman spectra of the SiMP/CNT wrapping 9:1 and SiMP/CNT wrapping 8:2 composites show specific peaks of SiMPs and SWCNTs. The result implies the co-existence of both SiMPs and SWCNTs in the SiMP/CNT wrapping composites. Interestingly, the SiMP/CNT wrapping composites show pronounced peaks from SWCNT but a weak Si peak. We consider that this result could be due to efficient SWCNT wrapping on the SiMPs. Compared to SiMP/CNT wrapping 8:2 composite, the SiMP/CNT wrapping 9:1 composite exhibits a greater intensity for the crystalline silicon peak around 500 cm−1 due to the larger amount of SiMP in the composite. The X-ray diffraction (XRD) pattern in Fig. 4b shows the characteristic crystalline peaks in the SiMP/CNT wrapping composites. The XRD peaks in the SiMP/CNT wrapping composites correspond to the XRD patterns of the SiMPs and SWCNTs.34,35 Specifically, the XRD patterns of the SiMPs can be indexed to Si (JCPDS 27-1402).34,36 Based on the XRD data, the SiMP/CNT wrapping composites exhibit noticeable SiMP peaks but show weak SWCNT peaks. The weak intensity of the SWCNT peaks could be due to the low amount of SWCNTs in the SiMP/CNT wrapping composites. To investigate the SWCNT content in the SiMP/CNT wrapping composite material, thermogravimetric analysis (TGA) analysis was conducted (Fig. 4c). Each sample was heated to 900 °C under air atmospheric conditions with a ramp rate of 10 °C min−1. Due to the oxidation of silicon at high temperatures in the air atmosphere, TGA curves of SiMP, SiMP/CNT wrapping 9:1, and SiMP/CNT wrapping 8:2 show gradual weight increases.11,37,38 In Fig. 4c, the TGA curves indicate that the amount of SWCNTs in the SiMP/CNT wrapping 8:2 and SiMP/CNT wrapping 9:1 composites is 16.9% and 8.7%, respectively. Accordingly, the SiMP content in SiMP/CNT wrapping 8:2 and SiMP/CNT wrapping 9:1 was estimated to be 83.1% and 91.3%, respectively. It can be seen that the amount of SWCNTs in SiMP/CNT wrapping 8:2 is about twice that in SiMP/CNT wrapping 9:1. Fig. 4d shows the N2 isotherm plots of SiMP, SWCNT, and SiMP/CNT wrapping composites along with their Brunauer–Emmett–Teller (BET) surface areas. The SiMP, SWCNT, SiMP/CNT wrapping 8:2, and SiMP/CNT wrapping 9:1 composite exhibit surface areas of 5.85, 39.55, 12.24, and 8.24 m2 g−1, respectively. Although both SiMP/CNT wrapping 8:2 and SiMP/CNT wrapping 9:1 show similar composite structures (Fig. 3d and e), they exhibit different BET surface areas. It can be found that the addition of a larger amount of SWCNTs results in a BET surface area increase. We consider that the increased content of mesh-like 2D CNT sheets in the SiMP/CNT wrapping composite could generate a larger surface area. In Fig. 4e, the Barrett–Joyner–Halenda (BJH) pore distribution data show that the SWCNTs have large pore volumes and a wide range of pore sizes. This result is consistent with the unique structure of the 2D CNT sheets in Fig. 1b–d. The segregated CNT network with inner voids between junctions and CNTs could affect the large pore volumes. With increasing SWCNT content, the SiMP/CNT wrapping composite displays a larger pore volume. The BET and BJH data are correlated with the morphological features of SiMP/CNT wrapping composites in Fig. 3d and e. Based on the results, we expected that the well-dispersed SWCNT content in the SiMP/CNT wrapping composites could strongly affect structural properties such as surface areas and porosity.
Each SiMP/CNT wrapping electrode was prepared using active material (SiMP/CNT wrapping):conductive additive (Super P):binder (CMC) in a weight ratio of 70:15:15. The electrochemical performances of the SiMP/CNT wrapping electrodes were evaluated in a galvanostatic mode in the potential range from 0.01 to 1.5 V versus Li/Li+. The SiMP/CNT wrapping electrode was fabricated in a half-cell configuration with lithium metal. Before the electrochemical test, the morphology and structure of the SiMP/CNT wrapping composite electrodes were investigated. The SEM images of the SiMP/CNT wrapping electrodes in Fig. S5† show the original structure of the active material, implying the structural stability of the SiMP/CNT wrapping after electrode fabrication. Generally, silicon electrodes are fabricated using an active material, a conductive additive, and a polymeric binder. In particular, the conductive additive plays an important role in providing a continuous conductive network within the electrode and improving the intrinsically low conductivity of silicon. In addition, in recent studies of Si/C composites, electrodes have also been prepared using a certain amount of conductive additive (Table S1†). As we used a conductive additive for the electrode fabrication, the resulting electrode exhibits a hybrid conductive network, which consists of carbon spheres and CNTs. The Super P particles are distributed with the SiMP/CNT wrapping composite in the electrode. When the SWCNT content was increased, the resulting SiMP/CNT wrapping 8:2 generated thick SWCNT coverage in the electrode (Fig. S5a and b†). Due to the larger amount of SWCNTs in the SiMP/CNT wrapping 8:2 composite, denser CNT networks were observed in the high-magnification SEM image in Fig. S5c†. However, the SEM image of the SiMP/CNT wrapping 9:1 composite-based electrode in Fig. S5d† shows a thinner 2D CNT wrapping network. Along with the mesh-like CNT sheets, the silicon microparticles underneath the CNT sheets were also observed. The result implies that the smaller amount of CNT dispersion generates porous CNT membranes, not dense CNT coverage, at the electrode level. The voids inside the electrode seem to decrease with increasing the amount of SWCNT dispersion in the composite. As a result, we consider that the SiMP/CNT wrapping composite structure could affect the electrode architecture. Additionally, this could be reasonable considering that the increased porosity in the electrode could facilitate inner void space toward volume changes of Si and accommodate facile lithium-ion diffusion in it.9
To investigate the electrochemical stability of the SWCNT dispersion, cyclic voltammetry (CV) of the SWCNT dispersion-coated electrode was conducted in a potential range of 0.01–3.0 V versus Li/Li+ (Fig. 5a). Fig. 5a shows the CV profile of the SWCNT dispersion, which lacks distinct redox peaks. The peaks in the potential range in the blue square box are related to the decomposition of electrolytes in the first cycle, which is usually observed in Si-based anode materials. Based on the weaker current response of the peaks, we considered the SWCNT dispersion to be suitable for the electrochemical test. In Fig. 5b and S6†, the CV curves of the SiMP/CNT wrapping 9:1 and SiMP/CNT wrapping 8:2 electrodes are shown. The CV analysis was conducted at the same scan rate of 0.2 mV s−1 for 5 cycles. The distinct anodic and cathodic peaks of Si are observed.3,4,39,40 In detail, the cathodic peaks around 0.2 and 0.01 V correspond to the lithiation of Si.9 In the anodic scan, two peaks at around 0.3 and 0.5 V are related to the de-lithiation process from the Li–Si alloy to amorphous silicon.39,41 The increase in the magnitude of the current peaks with subsequent scan cycles could be due to an Si activation process in the subsequent cycles, implying that more Si reacts with lithium in each cycle.42 Fig. 5c shows the galvanostatic charge and discharge profiles of the SiMP/CNT wrapping electrodes. The initial charge/discharge capacities of the SiMP/CNT wrapping 9:1 and SiMP/CNT wrapping 8:2 electrodes at 0.1 A g-1 are 3160.7 mA h g−1/3469.1 mA h g−1 and 2376.6 mA h g−1/2682.9 mA h g−1, respectively. The corresponding initial coulombic efficiency of the SiMP/CNT wrapping 9:1 and SiMP/CNT wrapping 8:2 electrodes is 91.11 and 88.58%, respectively. Overall, the SiMP/CNT wrapping 9:1 electrode delivered a higher specific capacity with high ICE. The higher ICE of SiMP/CNT wrapping 9:1 could be due to the relatively lower surface area of the composite (Fig. 4d).9,43 According to Fig. 4d, the BET surface area of SiMP/CNT wrapping 9:1 and SiMP/CNT wrapping 8:2 is 8.24 and 12.24 m2 g−1, respectively. The large surface area of the composite could result in increased electrolyte consumption and more SEI layer formation, resulting in low initial coulombic efficiency.44–46 The result implies the superior electrochemical performance of the SiMP/CNT wrapping 9:1, even with a smaller amount of SWCNTs. The better electrochemical performance of the SiMP/CNT wrapping 9:1 electrode is attributed to the optimal structural properties of thin 2D SWCNT wrapping on the SiMPs. Compared to the dense and thick SWCNT layers in the SiMP/CNT wrapping 8:2 composite, the mesh-like CNT wrapping on the SiMPs and the porous SiMP/CNT wrapping 9:1 electrode structure could offer sufficient inner voids at the electrode level. This could be beneficial for facile lithium-ion diffusion.40 As a result, we consider that the severe coverage derived from the larger amount of SWCNT dispersion in the SiMP/CNT wrapping 8:2 electrode could hamper the electrochemical activity of the SiMPs. In Fig. 5d, the rate performances of the SiMP/CNT wrapping electrodes at various C-rates are shown. The SiMP/CNT wrapping 9:1 electrode exhibits 3205.6, 3045.5, 2753.8, 2526.6, 2084.2, and 3173.3 mA h g−1 in the first step for each C-rate at 0.2, 0.5, 1.0, 1.5, 2.0, and 0.2 A g−1. The SiMP/CNT wrapping 8:2 electrode delivers 2514.6, 2313, 2113.1, 1888, 1588.1, and 2557.4 mA h g−1 under the same conditions. The corresponding galvanostatic charge and discharge profiles at various C-rates for the SiMP/CNT wrapping 9:1 and 8:2 electrodes are shown in Fig. S7a and b†. Despite its relatively lower amount of SWCNTs, SiMP/CNT wrapping 9:1 exhibits higher specific capacities at the various C-rates, which is attributed to its optimal structural properties. Due to the efficient CNT wrapping, the electrical isolation of the SiMPs could be effectively suppressed. SiMP/CNT wrapping 8:2 shows good rate capability at high current densities because of its larger amount of SWCNTs. Furthermore, the thick 2D CNT sheets in the SiMP/CNT wrapping 8:2 composite could ensure improved structural stability of the conductive network. As for the lower specific capacities of SiMP/CNT wrapping 8:2, we consider that the dense CNT coverage on the SiMP/CNT wrapping 8:2 electrode could reduce lithium-ion transport into the active materials, resulting in lower specific capacities (Fig. 5d). In this regard, SiMP/CNT wrapping 9:1 with a porous electrode structure provides the optimized conditions for electrochemical performance with facile lithium-ion access. To understand the better electrical performance of the SiMP/CNT wrapping 9:1 electrode, we investigated the kinetics of the SiMP/CNT wrapping composites. In Fig. 5e, the CV curves of the SiMP/CNT wrapping 9:1 and SiMP/CNT wrapping 8:2 electrodes at different scan rates (0.1–1.0 mV s−1) are shown. As expected, the SiMP/CNT wrapping 9:1 electrode exhibits an increased magnitude of current response in the CV data compared to that of the SiMP/CNT wrapping 8:2 electrode. Interestingly, neither the SiMP/CNT wrapping 9:1 nor the SiMP/CNT wrapping 8:2 electrodes showed distinct anodic peaks at the various scan rates. We expect that this could be due to fast scan rate changes from 0.1 mV s−1 to 1.0 mV s−1. These results have been observed in Si-based anode materials in other studies.8,47,48 In addition, the small changes in the CV profiles and peak position deviation in Fig. 5e could be the result of electrochemical polarization.49 The corresponding plots of the anodic and cathodic peak currents (Ip) against the square root of the scan rate of the SiMP/CNT wrapping 9:1 and SiMP/CNT wrapping 8:2 electrodes under different scan rates are shown in Fig. 5f. The redox kinetics of both electrodes are analyzed using the Randles–Sevcik eqn (1).50
Ip = (2.69 × 105)n1.5ADLi0.5v0.5CLi+ | (1) |
In the equation, Ip, n, A, DLi, v, and CLi+ stand for the peak current, the number of transferred electrons, electrode surface area, diffusion coefficient, potential scanning rate, and lithium concentration in the electrolyte, respectively.50 The results show a linear relationship between the peak currents and the square root of scan rate (Fig. 5f). Based on the CV performance in Fig. 5e, we found that the SiMP/CNT wrapping 9:1 electrode exhibits better kinetics, implying the better electrochemical performance of SiMP/CNT wrapping 9:1. The cycling performance of the SiMP/CNT wrapping electrodes is shown iN Fig. 5g. The SiMP/CNT wrapping 9:1 electrode exhibits higher specific capacities than that of the SiMP/CNT wrapping 8:2 electrode for 100 cycles. In the cycling performance of the SiMP/CNT wrapping 9:1 electrode, there are small capacity fluctuations, although this was not observed in the SiMP/CNT wrapping 8:2 electrode. This result implies that the higher content of SWCNTs in the SiMP/CNT wrapping 8:2 electrode ensures good structural stability. After 100 cycles, the SiMP/CNT wrapping 9:1 and SiMP/CNT wrapping 8:2 electrodes show capacity retention of 85.87 and 93.68%, respectively. In the SiMP/CNT wrapping composite, the SWCNTs, with superior mechanical stability, could ensure a stable structural network. Therefore, we consider that a larger amount of CNTs in the composite could improve the structural integrity against the volume changes of Si upon repeated charge and discharge cycling. According to previous studies, both initial and later-cycle coulombic efficiencies are regarded as important parameters for battery performance evaluation.6,51 The corresponding coulombic efficiency trends of cycling performance are shown in Fig. 5h. With high initial coulombic efficiencies, the SiMP/CNT wrapping 9:1 and SiMP/CNT wrapping 8:2 composites exhibit good later-cycle coulombic efficiencies of almost 98–99%. The improvement of early- and later-cycle coulombic efficiencies could be affected by stable SEI formation. Furthermore, the robust 2D CNT wrapping on the SiMPs might prevent uncontrolled SEI formation derived from repeated Si pulverization during volume changes.6 As a result, the SiMP/CNT wrapping 9:1 composite with thin 2D CNT wrapping exhibits high initial and later-cycle coulombic efficiencies along with stable SEI layer formation. In addition, a galvanostatic intermittent titration technique (GITT) test was conducted for the SiMP/CNT wrapping 9:1 and SiMP/CNT wrapping 8:2 electrodes (Fig. S8†).3,8 According to Fig. S8a†, the SiMP/CNT wrapping 9:1 electrode had a lower overpotential than that of the SiMP/CNT wrapping 8:2 electrode, resulting in better dynamic behavior.52–54 The magnified GITT profile in Fig. S8b† indicates lower polarization and internal resistance for the SiMP/CNT wrapping 9:1 electrode, which could be due to its optimal material and electrode structure.52 The diffusion coefficient of Li+ was calculated based on eqn (S1).† The lithium-ion diffusion kinetics of the SiMP/CNT wrapping 9:1 electrode are comparable to that of the SiMP/CNT wrapping 8:2 electrode (Fig. S8c†). The electrochemical performance of our work was further compared with other studies of SiMP/carbon composites in Table S1†. We found that the material in our work exhibits high initial capacities with superior ICE and comparable capacity retention due to efficient the SiMP/CNT wrapping composite structure.
To elucidate their electrochemical performance, electrochemical impedance spectroscopy (EIS) testing was conducted for the SiMP/CNT wrapping electrodes (Fig. 6a and b). In an attempt to prevent the influence of the lithium metal, each electrode was tested as a symmetric cell.9,39,40 Both SiMP/CNT wrapping 9:1 and SiMP/CNT wrapping 8:2 electrodes were tested in a galvanostatic mode at 1 A g−1 for 20 cycles. After cycling, the resulting 20-cycle electrodes were prepared with a state-of-charge (SoC) of 50% because the lithiated state of Si could influence the internal resistance. The corresponding equivalent circuits are shown in Fig. 6c and d. In Fig. 6a, the SiMP/CNT wrapping 9:1 and SiMP/CNT wrapping 8:2 electrodes show comparable impedance spectra for the initial state. The parameters Rs, RSEI, and Rct correspond to solution resistance, SEI layer resistance, and charge-transfer resistance, respectively. We compared the Nyquist plots of the SiMP/CNT wrapping 9:1 and SiMP/CNT wrapping 8:2 electrodes in Fig. 6a and b. In the initial state before cycling, the Rs and Rct of the SiMP/CNT wrapping 9:1 electrode are 3.40 ± 0.13 Ω and 3.01 ± 0.13 Ω, respectivelY (Fig. 6a). These parameters are smaller than those of the SiMP/CNT wrapping 8:2 electrode, which has an Rs and Rct of 4.91 ± 0.04 Ω and 3.31 ± 0.04 Ω, respectively (Table S2†). The smaller internal resistance of the SiMP/CNT wrapping 9:1 electrode is attributed to the optimal structural properties of the composite and electrode. After 20 cycles, each electrode was assembled as a symmetric cell for EIS analysis. From Fig. 6b and Table S2†, the Rs, RSEI, and Rct of the SiMP/CNT wrapping 9:1 and SiMP/CNT wrapping 8:2 electrodes are 2.69 ± 0.38 Ω, 7.50 ± 4.57 Ω, and 22.67 ± 7.71 Ω and 5.01 ± 0.16 Ω, 14.45 ± 3.75 Ω, and 29.83 ± 14.05 Ω, respectively. The smaller internal resistances of the SiMP/CNT wrapping 9:1 electrode after 20 cycles are attributed to the stable SEI formation and optimal electrode structure. Furthermore, the evenly distributed conductive additive in the electrode with a hybrid conductive network could result in reduced resistance. Compared to the SiMP/CNT wrapping 9:1 electrode, the SiMP/CNT wrapping 8:2 electrode exhibits slightly larger internal resistances. To investigate the structural stability of the SiMP/CNT wrapping electrodes after cycling, we conducted SEM analysis on cycled electrodes (Fig. 6e–h).55 Both the SiMP/CNT wrapping 9:1 and SiMP/CNT wrapping 8:2 electrodes exhibit smooth surfaces in Fig. 6e and g. As shown in Fig. 6g, the cycled SiMP/CNT wrapping 9:1 electrode shows a stable electrode surface. The well-preserved electrode structure was observed in a low-magnification SEM image. Therefore, we consider that the electrode was also preserved during repeated cycles. Interestingly, the high-magnification SEM images of the cycled electrodes show different structural properties (Fig. 6f and h). In the case of the SiMP/CNT wrapping 8:2 electrode, the cycled electrode shows thick SWCNT coverage on the SiMPs (Fig. 6f). Interestingly, the CNT networks are firmly attached to the SiMPs after cycling. In addition, the dense CNT-sheet-wrapped SiMPs are observed in the high-magnification SEM images of the cycled SiMP/CNT wrapping 8:2 electrode in Fig. 6f. The morphology of the SiMP/CNT wrapping 9:1 composite is also clearly shown in Fig. 6h. In the high-magnification SEM image, the morphology of the cycled SiMP/CNT wrapping 9:1 composite resembles insects captured by the lobes of a Venus flytrap. As the SWCNT sheets effectively wrap the silicon microparticles, the SiMPs could exhibit good electrochemical performance by taking advantage of the enhanced mechanical stability against Si volume changes and improved electrical conductivity. Due to the efficient 2D CNT sheet wrapping structure using well-dispersed SWCNTs, the silicon microparticles could maintain electrochemical activity during cycling without electrical isolation or detachment from the electrode (Fig. 7a).6 In Fig. 7b–e, TEM images of cycled SiMP/CNT wrapping electrodes are shown. For the cycled SiMP/CNT wrapping 8:2 electrode, dense and thick 2D CNT sheet coverage of the SiMPs is observed (Fig. 7b–c). In contrast, the cycled SiMP/CNT wrapping 9:1 electrode shows relatively thinner 2D CNT sheets due to the lower amount of SWCNT dispersion used for fabrication (Fig. 7d and e). After repeated cycling, the CNT wrapping is still seen in the TEM images, proving the excellent structural integrity of the CNT network. Furthermore, the embedded silicon microparticles in the SiMP/CNT wrapping composite are observed, indicating the efficient structural stability and conductive network in the composite. In Fig. S9a and b†, the magnified TEM images show the surface of the cycled SiMP/CNT wrapping 8:2 and SiMP/CNT wrapping 9:1 active material. We consider that the SEI layer is mainly expected to form on the 2D CNTs, which is the outer surface of the SiMP/CNT wrapping composites. Therefore, the SEI layer formation on the CNTs could result in high initial coulombic efficiency with a stable SEI layer.6,51 In addition, the robust CNT wrapping could prevent uncontrolled SEI layer formation upon repeated pulverization of the SiMPs. Compared to that in Fig. S9b†, the magnified TEM image of cycled SiMP/CNT wrapping 8:2 in Fig. S9a† shows a thicker SEI layer. This could be due to the larger surface area of the SiMP/CNT wrapping 8:2 composite (Fig. 4d).
Footnote |
† Electronic supplementary information (ESI) available: Fig. S1–S9, eqn (S1), Tables S1 and S2 as described in the manuscript. See DOI: https://doi.org/10.1039/d2ra07469a |
This journal is © The Royal Society of Chemistry 2023 |