Yufeng Zhanga,
Wenxiong Zhaoa,
Qiuchen Wuab,
Xinlu Linab,
Ziyao Zhuab,
Ruchun Liab,
Yuhang Liuab,
Kai Huanga and
Xiangxin Liu*ab
aThe Key Laboratory of Solar Thermal and Photovoltaic System, Institute of Electrical Engineering, CAS, Beijing 10019, China. E-mail: shinelu@mail.iee.ac.cn
bUniversity of Chinese Academy of Sciences, Beijing 10049, China
First published on 23rd March 2023
The Ga doped ZnO (GZO) film is one of the promising alternative films to replace ITO film, but its properties suffer from degradation when it is deposited under oxygen-rich conditions. This degradation has been investigated by depositing the films under different oxygen partial pressures. XRD results showed that all GZO films had wurtzite structure and the lattice parameter-c contracted when oxygen was introduced into the argon deposition atmosphere, but the parameter-c nearly remained constant when oxygen partial pressures were further increased. The contraction of parameter-c was caused by the increasing concentrations of VZn (Zn vacancy). It was the first time to observe that the impurity phase of Ga2Zn6O9 appeared and disappeared in GZO films during the increase of oxygen partial pressures. Analogously, conductivity decayed and optical bandgap decreased abruptly as oxygen was introduced, which enhanced self-compensation of donors and acceptors. The energy band structures of GZO and ZnO films were determined by using UPS, and the results showed that oxygen had little effect on the electron affinity of the GZO film, but a significant difference in electron affinity between the ZnO and GZO films was observed. This result indicated that although the electron affinity of ZnO could be effectively tuned by doping with Ga, it remained quite stable for GZO under oxygen-rich conditions.
However, GZO film has been proved to be heavily impacted by the oxygen during the growth of films. M. H. Lee et al. investigated the intrinsic defects of GZO by adopting ab initio methods, and the results showed that the formation energy (Ef) of GaZn was −3.7 eV in an oxygen-rich condition, while it increased to −0.21 eV in an oxygen-poor condition. The decline of intrinsic defect formation energies was Ef (VZn) < Ef (Oi) < Ef (VO) in oxygen-rich conditions, but it was Ef (VO) < Ef (VZn) < Ef (Oi) in oxygen-poor conditions.6 C. S. Lee et al. prepared Zn0.96Ga0.04O films on the quartz substrates, and the film growth was carried out in a mixed gas of Ar and O2, with the O2/Ar + O2 ratios ranging from 0.0 to 1.0. The experimental results showed that with the addition of the oxygen in the growth ambient, the resistivity abruptly increased from 2.52 × 10−4 Ω cm to 0.295 Ω cm, which was derived from the sudden reductions in the electron density and mobility because of the compensation via GaZn–VZn complexes.5 The self-compensation effect between VZn defects energy level and Ga3+ doped energy level has been also revealed in ZnO matrix by D. C. Look.7
The GZO thin film transistors were fabricated by X. Q. Li et al., and the GZO (2 wt% Ga) film was deposited at variable oxygen pressure. The experimental results showed that a small amount of oxygen caused a decrease in oxygen deficiency of the film, which reduced electron trapping and facilitated carrier transport. However, excessive oxygen caused an increase in the receptor complex such as GaZn–Oin and GaZn–VZn.8 W. S. Noha et al. prepared the ZnO:Ga0.01P0.04 thin films by the PLD method, and the film exhibited a transition from n-type to p-type conductivity above the oxygen partial pressure of approximately 200 mTorr.9
In this work, the GZO films were prepared by using RF sputtering under various oxygen partial pressures, and the band structure, impurity and opto-electrical properties were investigated.
Sample name | G1 | G2 | G3 | G4 | G5 | G6 |
---|---|---|---|---|---|---|
Oxygen partial pressure/Pa | 0 | 0.065 | 0.125 | 0.182 | 0.235 | 0.286 |
The structures of thin films were characterized by using X-ray diffraction (XRD), and the chemical states of the film surface were investigated by using X-ray photoelectron spectroscopy (XPS) after sputter etching of the film surface. The morphology was carried out by using scanning electronic microscopy (SEM). The electrical properties were analyzed by using the Hall effect measurement, and the transmittance of the thin films in the wavelength range of 300–900 nm was measured by using an ultraviolet-visible spectrophotometer.
However, the intensities of both (0 0 2) and (0 0 4) peaks decreased with increasing oxygen partial pressure due to a reduction in film thickness and the crystallinity degradation.
In Fig. 1(b) the value of parameter-c for G1 film was 5.12 Å, which was much smaller than that of pure ZnO (c = 5.21 Å). This suggested that the Ga ions effectively doped into the lattice of ZnO matrix because of the smaller ionic radius of Ga and the shorter bond with oxygen.
As the oxygen partial pressure increasing to 0.065 Pa in G2 film, the positions of (0 0 2) and (0 0 4) peaks sharply increased, and the value of parameter-c decreased to 5.10 Å. Although the oxygen partial pressure continued to increase, this value nearly remained unchanged.
The decrease in the value of parameter-c might be due to the increasing concentration of VZn because of its lowest formation energy in an oxygen-rich condition.6 The high concentration of VZn would induce a great Coulomb force of attraction among the ions around it, which may cause crystal distortion and contraction of crystal lattice.
The strain values of GZO films could be calculated by the eqn (1):11,12
(1) |
(2) |
G1 | G2 | G3 | G4 | G5 | G6 | |
---|---|---|---|---|---|---|
ε (%) | −1.68 | −2.05 | −2.05 | −2.09 | −2.07 | −2.03 |
σ (GPa) | 3.85 | 4.68 | 4.68 | 4.76 | 4.72 | 4.63 |
The impurity phases were analyzed by enlarging the XRD patterns. As shown in Fig. 2, there was no peak at the 2θ range of 30°–33° in G1, however, at the oxygen partial pressure of 0.065 Pa (G2), two new peaks appeared at 31.14° and 33.09°, which were indicated by arrows. The new peaks could be indexed to the orthorhombic structure of Ga2Zn6O9 (ICSD #173602).13 The intensity of each new peak was much lower than that of (0 0 2) peak from GZO, which indicated that the amount of the impurity was very small.
When the oxygen partial pressure increased to 0.182 Pa (G4), another new diffraction peak appeared at 31.16°, and it belonged to the (1 0 0) plane of GZO. The intensities of peaks belonging to Ga2Zn6O9 gradually diminished and disappeared when the oxygen partial pressure was 0.235 Pa (G5) or higher. The impurity of Ga2Zn6O9 appeared and disappeared during the increase of oxygen partial pressure, which implied that Ga ions might extract from the lattice of ZnO first and existed in the form of an amorphous state at higher oxygen partial pressure finally. This result suggested the effective doping of GaZn in lattice of ZnO matrix reduced. The parameter-c was almost unchanged in oxygen-rich conditions due to a small trace of impurity. Moreover, the diffraction peaks from Ga, Ga2O3 or ZnGa2O4 were not detected.
The defects and chemical states of GZO films were characterized by XPS. Ga-2p3/2 peaks were decomposed into two peaks at 1117.9 eV and 1118.6 eV, as shown in Fig. 3(a) and (b). The peak at 1117.9 eV was derived from the GaZn–O bonds, in which Ga atoms substituted for Zn atoms in ZnO matrix, while the peak at 1118.6 eV could be attributed to the Ga–O bonds duo to GaOx sub-oxides and oxides in intra-grain congregation or grain-boundary segregation.14–16 The intensity for the Ga-2p3/2 peak at 1117.9 eV decreased while it increased for the Ga-2p3/2 peak at 1183.6 eV. The results suggested that a number of Ga ions which replaced Zn in ZnO matrix were lost from the lattice of the matrix and might exist in the form of GaOx sub-oxides with the increasing oxygen partial pressure.
Fig. 3 XPS spectra of Ga–2p3/2 peaks for: (a) G1 film; (b) G6 film, and O-1s peaks for: (c) G1 film; (d) G6 film. |
The asymmetric peak observed in the O-1s spectrum of G1 film could be fitted by three types of peaks, as shown in Fig. 3(c). The lowest binding energy peak of O-1s, centered at 530.6 eV, was marked as O3rd and derived from the bonds between O2− and metal ions (Zn2+ and Ga3+).17,18 The middle peak at 531.3 eV (O2nd) corresponded to oxygen vacancies in the G1 film.19,20 The highest binding energy at 532.2 eV was marked as O1st, which was related to oxygen near surface, such as O–H bonds.21,22 In comparison with the G1 film, the O1st, O2nd and O3rd peaks of G6 film were located at 530.2 eV, 531.3 eV and 532.3 eV in Fig. 3(d). The intensity of the O2nd peak was proportional to the concentration of oxygen vacancies.23 Peak intensity ratio of O2nd/Ototal was 26.7% for G1 film, but it decreased to 21% for G6 film, which indicated that the VO concentration in GZO film obviously decreased at the oxygen partial pressure.
The effect of oxygen partial pressure on the morphology of the GZO films was analyzed by using SEM. As shown in Fig. 4, the surface of the G1 film appeared compact and crack-free. In contrast, G2 film exhibited wide and deep boundaries, which became narrower in G3 film. The G4 film showed large grains with a tetrahedral shape, as indicated by arrows, and the number of these grains increased with increasing oxygen partial pressure.
In general, the compact surface of G1 film turned into grains with a lot of boundaries in oxygen-rich conditions. The results suggested the nucleation and growth process during the formation of GZO films might be affected by oxygen, which reduced the island size in the coalescence stage.24,25 By comparison, it has been observed that the grain size of ZnO:Mg film decreased with the increasing oxygen partial pressure.26
Additionally, the tetrahedral grains could be caused by abnormal grain growth. In the oxygen-rich conditions, the mobility of boundary migration was limited, but some grain boundaries might have overcome the pinning effect and grown into larger sizes compared to other boundaries that were still pinned.27
Fig. 5 Resistivity, carrier concentration and Hall mobility of GZO films under various oxygen partial pressures. |
The high n-type carrier concentration (ntotal) for the G1 film was due to the high concentrations of GaZn and VO donor defects. The carrier concentration was reduced mainly due to the decrease of VO concentration and the increase of VZn concentration, which acted as compensating intrinsic defects.5
Fig. 7(a) and (b) showed the variation of the optical bandgap with increasing oxygen partial pressures. The bandgap of the G1 film was 3.47 eV and decreased rapidly to 3.31 eV under an oxygen partial pressure of 0.065 Pa (G2). The optical bandgaps then remained almost constant at 3.31 eV with increasing oxygen partial pressure, which were larger than that of the pure ZnO film (3.26 eV).
Fig. 7 The (a) and (b) showed the optical bandgap of GZO (ball) varied with the O2 partial pressure and the value of ZnO was indicated by the symbol of star. |
The optical bandgap of the G1 film was the largest due to the Burstein–Moss (B–M) effect, which described the blue-shift of the optical bandgap energy. The relationship between the broadening of the optical band gap (ΔEg) and carrier concentration (n) could be expressed by eqn (3):3,29
(3) |
The UPS spectra for G1, G6, and ZnO films were shown in Fig. 8(a)–(c), respectively. The error tolerances in our analyses were ±0.15 eV. The VBM was determined by the cross point at the linear extrapolation of the edge of UPS and the baseline (X-axis). The band structures of G1, G6 and ZnO were shown by Fig. 8(d)–(f), respectively, by combining them with the optical band gap. The electron affinity of G1 was 3.57 eV, while it was 3.54 eV for G6. The result suggested that oxygen partial pressure had almost no effect on the electron affinity, which was a key parameter in band alignment of device consisting with multilayer films. For comparison, the electron affinity of ZnO was as high as 4.49 eV, which was much larger than G6, although both ZnO and G6 were insulated. The experimental results showed that the electron affinity of ZnO could be effectively tuned by doping Ga, but electron affinity of GZO had almost not been affected by oxygen partial pressure.
Fig. 8 (a)–(c) were UPS spectra which correspond to G1, G6 and ZnO films. (d)–(f) Were sketches of band structures which correspond to G1, G6 and ZnO films. |
The opto-electrical properties of GZO films deposited at different oxygen partial pressures were measured. The resistivity increased from 4.5 × 10−4 Ω cm to 52.3 Ω cm when the oxygen partial pressure increased from 0 to 0.286 Pa, mainly due to the decrease of VO concentration and the increase of VZn concentration, which acted as compensating intrinsic defects. Meanwhile, the optical bandgap of GZO film decreased with the increase in oxygen partial pressure from 3.47 eV to about 3.30 eV. The results showed that the conductivity and optical bandgap of GZO film were easily affected by oxygen partial pressure. Additionally, the electron affinities were 3.57 eV and 3.54 eV for G1 and G6, respectively, and it was proved that the oxygen partial pressure had almost no effect on the electron affinity of GZO film in oxygen-rich condition. For comparison, the electron affinity of ZnO film was 4.49 eV, which suggested that Ga played an important role in tuning electron affinity of ZnO film.
This journal is © The Royal Society of Chemistry 2023 |