DOI:
10.1039/D3RA05873E
(Paper)
RSC Adv., 2023,
13, 31167-31175
Concentration quenching inhibition and fluorescence enhancement in Eu3+-doped molybdate red phosphors with two-phase mixing†
Received
28th August 2023
, Accepted 13th October 2023
First published on 1st November 2023
Abstract
Red phosphor plays a crucial role in improving the quality of white light illumination and backlight displays. However, significant challenges remain to enhance red emission intensity in different matrix materials. Herein, a class of two-phase mixing red phosphors of NaIn1−x(MoO4)2:xEu3+ (NIMO:xEu3+) has been successfully prepared by the traditional high-temperature solid-state reaction method. The coordination environment, phase structure, excitation and emission spectra, fluorescence kinetics, and temperature-dependent luminescence properties of the system have been studied comprehensively. It is worth mentioning that the red emission intensity continues to increase with the increased Eu3+ doping concentration, and the fluorescence lifetimes remain unchanged. These extraordinary phenomena mainly stem from the special concentration quenching mechanism in such two-phase mixing material, namely, the increased lattice interface barriers from Eu six-coordinated units and Eu eight-coordinated units can effectively block the non-radiation by enlarging the average distance between luminescent centers. The improved fluorescence thermal stability and suppressed non-radiative transition rate in NIMO:40%Eu3+ sample are further proving regulatory role of lattice interface barriers. In addition, a warm white light-emitting diode (LED) is successfully fabricated, exhibiting Commission Internationale de l'Eclairage (CIE) coordinates of (0.343, 0.335), a color rendering index (CRI) of 92.1, and a correlated color temperature (CCT) of 5013 K, showing significant application prospects for high-quality lighting devices.
1. Introduction
In recent years, inorganic luminescent materials have received increasing attention from scholars due to their widespread applications in lighting, displays, optical communication, solar cells, biological detection, and other fields.1–7 Currently, a popular lighting solution for producing white light is the utilization of commercial blue fluorescent LED chips combined with yellow light YAG:Ce3+ phosphors.8–10 However, the problems of high color temperature and low color rendering index need to be further solved in the warm white lighting field due to the lack of red components.11 With further research, Mn4+ doped fluoride red light material as an excellent candidate is gradually being utilized in the production of white LEDs to make up the shortcoming, but poor moisture resistance is the key factor restricting its promotion and application.12,13 Therefore, it is still necessary to explore alternative stable and efficient red light materials for warm white LEDs.
Eu3+ ions, with a typical 4f–4f electronic layer transition, are minimally influenced by external electromagnetic fields and demonstrate highly efficient near-ultraviolet excitation and conversion into red emission.14 In recent years, Eu3+ activated oxide red light materials play an important role in the production of near-ultraviolet (NUV) excited white LED devices, because of its excellent physicochemical stability and favorable luminescent performance. Eu3+ doped red phosphors have been extensively studied, such as in silicate, borate, vanadate, phosphate, molybdate, tungstate, organic complexes and other systems.15–20 Considering the luminous efficiency, the number of effective Eu3+ centers is one of the important influencing factors. In general, the cross-energy transfer (CET) among Eu3+ ions increases becomes more serious as the luminescent centers increases (doping concentration increases), leading to the occurrence of concentration quenching effects. Many studies have clarified that the CET relation can be effectively changed through the regulation of micro-structure, such as in La2W2O9:Eu3+, Ca(Sr)Al12O19:Eu3+, MBaY(BO3)2:Eu3+ (M = Na, K), KLa1−x−y(MoO4)2−z(WO4)z:xEu3+/yDy3+, CaMoO4:Eu3+/Na+.21–25 In these numerous methods, entering a reasonable crystal field distortion by replacing non-rare-earth ions with rare-earth luminescent centers is an effective approach for improving luminescence performance. For LaSc3(BO3)4:Eu3+ red light material, the host lattice gradually shifts from phase α to β with the increasing Eu3+ concentration. At the same time, due to the increasing luminescence center spacing, there is a significant improvement in luminescence efficiency, while also exhibiting excellent luminescent thermal stability.26,27 In certain materials, there exists a notable separation between the positions occupied by luminescence centers. This spatial disparity becomes evident in instances such as the extended distance between emission centers in phosphors like Li3BaSrLa3(MoO4)8:Eu3+ and LiCaLa(MoO4)3:Eu3+. It is crucial to underscore that this spatial separation plays a pivotal role in influencing both emission efficiency and thermal stability. The discernible impact on these properties emphasizes the intricate relationship between the arrangement of luminescence centers and the overall performance characteristics of the aforementioned phosphors.28,29 Our recent study has found that in the non-equivalent substituted SrWO4:Eu3+ phosphor, a second phase structure of Eu2W2O9 appears as the Eu3+ concentration increases and an associated luminescence enhancement presents when the Eu3+ concentration reaches a certain level.30 Therefore, further exploration is needed to improve the luminescence efficiency and stability of red light materials by using the strategies of changing host structure.
In this work, a series of NIMO:xEu3+ (x = 10–90%) red fluorescent powders are prepared using a high-temperature solid-state reaction method. Accompanied by significant differences in atomic radius between Eu3+ and In3+ ions, two crystal structures of Eu3+, six-coordinated and eight-coordinated, are formed in host material. The spectral analysis indicates that the typical luminescence concentration quenching phenomenon of Eu3+ is suppressed while obtaining enhanced luminescence. A novel concentration quenching mechanism on regulating the non-radiative transition rate in two-phase mixing material is suggested to explain the enhancement of luminescence, invariant fluorescence lifetimes, and improved luminescence thermal stability. Moreover, the prepared white LED exhibits superior luminous performance on CIE of (0.343, 0.335), CRI of 92.1 and CCT of 5013 K, which can meet the requirements of high-quality lighting applications.
2. Experimental section
2.1 Sample preparation
The raw materials, including Na2CO3 (99.99%), In2O3 (99.99%), MoO3 (99.99%), and Eu2O3 (99.99%), are used to prepare NIMO:xEu3+ phosphors through a high-temperature solid-state method. Chemical ratios dictate the precise weight of each raw material used, and samples with varying doping ratios (x = 10–90%) are prepared. These samples are then finely ground in a mortar for 30 minutes before being placed in an alumina corundum crucible. The mixture is heated at a rate of 3 K min−1 in a muffle furnace to 923 K and calcined for 8 hours. Following cooling to room temperature, the samples are retrieved for grinding and subsequent qualitative and quantitative analysis. The preparation of pc-LED is achieved by mixing a certain proportion (1:1) of phosphors with UV curing adhesive, and then coating it on a NUV LED chip.
2.2 Sample characterization
A CuK α radiation source was used with an X-ray diffractometer (XRD), at a tube current of 40 mA and tube voltage of 40 kV, to analyze the phase structure of samples. The Beijing Zhuolihanguang Instrument Co., Ltd provided the OmniFluo900 fluorescence spectrometer to conduct excitation, emission, and fluorescence lifetime tests on the samples using a 75 W xenon lamp and 20 Hz pulse laser. The fluorescence spectrometer was combined with the Oxford Low Temperature Opto-electronic Test and Analysis System to investigate the thermal stability index of the sample, with a sampling interval of 25 K in a variable temperature environment of 100–500 K. In addition, absolute quantum yield measurements were conducted using the Edinburgh Instruments FS5 fluorescence spectrometer equipped with an attached integrating sphere module. Electroluminescence spectra of the pc-LEDs were performed by the Auto-Temperature LED Opto-electronic Analyzer of EVERFINE.
3. Results and discussion
3.1 Crystal structure analysis
The cell parameters of NIMO can be obtained from the standard structure in the inorganic crystal structure database (ICSD): the space group is P1, a = 7.29 Å, b = 7.29 Å, c = 15.06 Å, α = 90.01°, β = 90.02°, γ = 99.11°, V = 788.93 Å3, Z = 4, belonging to the triclinic system.31 In3+ (CN = 6, r = 0.81 Å) is less than Eu3+ (CN = 6, r = 0.947 Å). The cell parameters for NaEu(MoO4)2 (NEMO) as follows: the space group is I4, a = 5.35 Å, b = 5.35 Å, c = 11.64 Å, α = 90°, β = 90°, γ = 90°, V = 332.76 Å3, Z = 2, belonging to the tetragonal crystal system.32 Eu3+ (CN = 8, r = 1.07 Å) is greater than In3+ (CN = 8, r = 0.92 Å). From Fig. 1(a), it can be seen that the NIMO unit cell contains six-coordinated [InO6] and four coordinated [MoO4], while the NEMO unit cell contains eight-coordinated [EuO8] and four-coordinated [MoO4]. As to NIMO hosts, In3+ ions are located in anti-centrosymmetric positions of the unit cell, substitution of Eu3+ ions can reduce the symmetry and breaks the parity prohibition, while causes energy absorption and emission. In contrast, In3+ ion replaces Eu3+ in the octahedral dodecahedron of the NEMO unit cell, not in the anti-symmetric center, while the weaker energy transfer occurs. It is reported that the probability of successful replacement of luminescent centers depends on the degree of difference in ion radius. The formula is as follows:33 |
| (1) |
where R1 represents the ionic radii of In3+ and R2 represents the ionic radii of Eu3+. According to formula (1), D1 = 18.4%, D2 = 13.7%, are all below 30%, representing the possibility of Eu3+ and In3+ effectively occupying two different structures. In addition, due to differences in coordination environment, the cell volume of NIMO is 2.37 times that of NEMO, it can be clearly known that when the crystal field undergoes severe distortion and changes, new CET relationship regulation laws will occur in such materials. In Fig. 1(b), it can be clearly seen that when the Eu3+ doping concentration is below 20%, the powders mainly exhibit diffraction peaks of NIMO with a PDF card no. 27-0713. However, as the Eu3+ doping concentration further increases, diffraction peak of NEMO with a PDF card no. 055-0992 appears and gradually strengthens. When the Eu3+ doping concentration exceeds 70%, the main manifestation is the diffraction peak of NEMO. In the field of materials science, research on the structural phase transition caused by the increase of doping components is very interesting.34 According to XRD analysis, there is a typical two-phase mixing and gradual transitions with varying Eu3+ concentrations in this material, which will become an important origin for regulation of emission properties.
|
| Fig. 1 (a) Schematic crystal structures of NIMO and NEMO. (b) XRD patterns of Eu3+ doped NIMO samples. | |
3.2 Concentration-dependent luminescence and dynamics properties
Eu3+ is one of the most popular red light emitting centers due to its typical 5D0–7F1,2 transitions. The photo-luminescence excitation (PLE) and emission (PL) spectra of Eu3+ doped NIMO are given in Fig. 2. In Fig. 2(a), the PLE spectrum contains a wide charge transfer band (CTB) and a series of narrow band absorption peaks. The broadband absorption peak range 260–360 nm with a central wavelength of 305 nm is attributed to the charge transfer from the 2p orbitals of O2− in MoO42− to the unfilled 4f orbitals in Eu3+. The stronger covalent bond between W and O reduces the probability of O2− migrating to Eu3+, showing a relatively weak charge absorption band.35 In addition, the narrow band absorption peaks range from 360–450 nm are derived from the transitions in 4f orbitals of Eu3+. Some strong peaks appear at 362 nm, 382 nm, 395 nm, 416 nm, and 465 nm, corresponding to transitions of 7F0–5D4, 7F0–5GJ/5L7, 7F0–5L6, 7F0–5D3 and 7F0–5D2, respectively. These wavelengths exactly match the emission wavelengths of near-ultraviolet and blue light chips, making them valuable in red and white LED applications. PLE spectra with different Eu3+ doping concentrations are presented in Fig. 2(b). It can be clearly seen that the CTB gradually undergoes a red shift, which is due to a shortening of the bond length between Eu and O as the crystal phase changes, resulting in a decrease of the energy needed to transfer electrons from the 2p orbital of O2− to the 4f orbital of Eu3+. This also corresponds to the experimental conclusion of XRD patterns. In contrast, the positions of a series of sharp absorption peaks remain constant due to energy level transitions within the 4f–4f orbitals. For better understanding of charge transfer process and energy level transitions, Fig. 2(c) presents the classical energy level diagram of Eu3+ ions with the main excitation and emission processes. In molybdate luminescent materials, when the excited state electron transitions to various energy levels from the ground state, the main emission peaks belong to 5D0–7FJ, which is due to the large phonon threshold of molybdate matrix and the high non-radiative transition rate between high-energy levels.
|
| Fig. 2 (a) PLE spectrum of NIMO:90%Eu3+ sample. (b) PLE spectrum of NIMO:xEu3+ with different Eu3+ doping concentrations. (c) Energy level diagram of Eu3+. (d) PL spectrum of NIMO:90%Eu3+ sample, inset is its CIE coordinate. (e) Emission peaks of NIMO:xEu3+. (f) Integrated intensity of NIMO:xEu3+ | |
In Fig. 2(d), the PL spectra of Eu3+ are measured at the excitation wavelength of 395 nm. It can be seen that all spectra exhibit narrowband emissions at 592 nm, 616 nm, 656 nm, and 702 nm, corresponding to transitions 5D0–7F1, 5D0–7F2, 5D0–7F3, and 5D0–7F4. It can be clearly seen that the electric dipole transition 5D0–7F2 is dominant and gradually enhances with increased Eu3+ concentration. The previous report have shown that the ratio of 5D0–7F2 to 5D0–7F1 not only determines the color of the emitted light but also reflects the local symmetry of Eu3+ 26. The calculation results in Fig. S1† indicates the ratios remain unchanged, which suggests that the increasing Eu3+ doping concentration does not alter the low inversion symmetry of Eu3+ from the octahedral and dodecahedral substitution and maintains stable color purity simultaneously.36,37 In the inset of Fig. 2(d), the CIE coordinates of NIMO:90%Eu3+ is (x, y) = (0.668, 0.332), similar to the internationally recognized standard for red color (0.666, 0.334). Moreover, the color purity of all samples is higher than 96% by calculation.38 In Fig. 2(e) and (f), the emission peaks and integral intensity of NIMO:xEu3+ with Eu3+ doping concentrations from 10% to 90% are measured and calculated. It is worth noting that the integral intensity of samples gradually increase with the enhanced Eu3+ doping concentrations, and no traditional concentration quenching phenomenon is observed.
In traditional luminescent materials, emitters can homogeneously disperse into the interior host matrix by replacing the equivalent ions that have similar ionic radii, the occurrence of concentration quenching is mainly due to the accelerated CET with closer distance between dopants.39 However, a different mode of energy transfer relationship on concentration quenching inhibition should be highlighted in NIMO:xEu3+, and the energy transfer relationship model is represented in Fig. 3. It can be clearly seen that, as the Eu3+ concentration increases, the second phase of NEMO gradually generates and manifolds. There exist three pathways for CET between emitters in such materials, namely Eu–Eu in the six-coordinated structure, Eu–Eu in the eight-coordinated structure, and Eu–Eu between the six-coordinated and eight-coordinated structures. According to Blasse's report, when the distance between emitters is less than 5 Å, energy transfer is prone to occur between them.40 On the contrary, when the distance is greater than 5 Å, energy transfer is less effective. In NIMO, if In3+ is completely occupied by Eu3+, the closest distance between emission centers is 5.8827 Å. But in NEMO, the closest distance between emission centers is 5.3470 Å. Therefore, the sustained fluorescence enhancement in NIMO:xEu3+ indicates that the average distance between Eu3+ emitters is increasing. It should be emphasized that the main contribution to increasing the average spacing comes from the increase in lattice interface barriers between six-coordinated Eu unit and eight-coordinated Eu unit. The increasing interface barriers can effectively block the CET between the two-phase structures and mount up the number of emitted photons for enhancing emission.41,42 In addition, it is observed that the emission intensity of NIMO:90%Eu3+ is about 1.3 times that of NEMO in Fig. S2,† indicating an efficient red light emission can be achieved under this CET mechanism. Moreover, the absolute quantum yield of the NIMO:90%Eu3+ phosphor is measured in Fig. S3† and a remarkable value of 90.87% is obtained under the excitation wavelength of 395 nm.
|
| Fig. 3 Schematic diagram of the energy transfer relationship in the NIMO:xEu3+. | |
In Fig. 4, the fluorescence lifetime curves are measured to investigate the microscopic population process of Eu3+ activators in NIMO:xEu3+ phosphors. Fig. 4(a) displays the fluorescence decay curve of NIMO:40%Eu3+ in 5D0–7F2 transition, which can be well fitted by the following first-order exponential equation:43
|
I(t) = Aexp(−t/τ)
| (2) |
where
I(
t) represents the luminous intensity at time
t,
A is a constant, and
τ is the average single photon fluorescence lifetime. The fitting result shows that the decay time constant is 402.3 μs. In
Fig. 4(b) and (c), it is interesting to find that all lifetimes of Eu
3+ doping concentrations ranging from 10% to 90% are almost unchanged and around 400 μs, this is also means that the total electron transition rates do not change with the variation of Eu
3+ doping concentrations. As is known that, the electron transition rate includes two parts: radiative transition rate and non-radiative transition rate. Generally, when the environment of the luminescent center is stable, the radiation transition rate remains almost constant, but the non-radiative transition rate is related to the change in crystal field. In NIMO:
xEu
3+, there are two main factors that affect non-radiative transition, one is the CET between Eu ions in the six-coordinated structure, the other is the CET between Eu in the six-coordinated structure and Eu in the eight-coordinate structure. In the six-coordinated structure of NIMO, the increasing Eu
3+ doping concentration can shorten the distance between them, while increasing the non-radiative transition rate. Complementarily, the lattice interface barriers related to Eu in the six-coordinated structure and in the eight-coordinated structure will also increase with the increasing Eu emitters, which can decrease the non-radiative transition rate by blocking the CET between them. The unchanged lifetimes in NIMO:
xEu
3+ indicate that the increasing non-radiative transition rate is equivalent to the decreasing value, and cancels out each other. To better understand the regulatory mechanism of non-radiative transition rate, a vivid schematic diagram is shown in
Fig. 4(d). Furthermore, the fluorescence lifetime of NEMO is measured and calculated as 336 μs in Fig. S4,
† indicating the serious non-radiative transition processes among their Eu emitters.
|
| Fig. 4 (a) Fluorescence decay curve of NIMO:40%Eu3+. (b) Fluorescence decay curves of NIMO:x%Eu3+. (c) Fluorescence decay time constants of NIMO:x%Eu3+. (d) Schematic diagram of non-radiative transition regulation mechanism in NIMO:x%Eu3+. | |
3.3 Temperature-dependent emission spectra and dynamics
As is well known, there is a strong dependence of luminescence intensity on environmental temperature, which is known as thermal-quenching effect. To reveal the thermal-quenching properties in the two-phase mixing NIMO:xEu3+ materials, the PLE and PL spectra of NIMO:xEu3+ (x = 10% and 40%) with the varying temperature range from 100 K to 500 K are displayed in Fig. 5(a) and (b). In Fig. 5(a), it can be seen that absorption bands of matrix in NIMO:40%Eu3+ have a red shift with the increasing temperature, which is due to the different sensitivity to temperature for the overlapping PLE spectra in the two-phase structures. In Fig. 5(b), it is evident that the PL intensity of NIMO:40%Eu3+ gradually decreases with increasing temperature, but the position and proportion of the emission peaks remain almost unchanged, indicating a good color thermal stability. As the PLE and PL spectra measured in Fig. S5,† if the luminous intensity at 300 K is used as a reference, when temperature rises to 400 K, the emission intensities of NIMO:10%Eu3+ and NIMO:40%Eu3+ remain at 53.5% and 76.3%, which indicates that sample with high Eu3+ doping concentration exhibits good luminescence stability. In Fig. 5(c), the activation energy is obtained by the following formula:44 |
| (3) |
where I0 represents the initial luminous intensity, ΔE is the thermal activation energy, k is the Boltzmann constant, T is the real-time temperature, and c is the constant. By fitting, the thermal activation energy of NIMO:10%Eu3+ and NIMO:40%Eu3+ are 0.327 eV and 0.388 eV. It can be seen that samples with higher doping concentrations have higher thermal activation energy, thus exhibiting good luminescence stability. It should be noted that the CET mainly occurs among the six-coordinated Eu3+ ions in NIMO:10%Eu3+ phosphor. But in NIMO:40%Eu3+, the gradually increasing lattice interface barriers can effectively block the CET, thereby inhibiting the thermal activation process of materials.
|
| Fig. 5 (a) Temperature-dependent PLE spectra of NIMO:40%Eu3+. (b) Temperature-dependent PL spectra of NIMO:40%Eu3+. (c) Temperature dependence of normalized integral intensities of NIMO:10%Eu3+ and NIMO:40%Eu3+. (d) Temperature-dependent fluorescence decay curves of NIMO:40%Eu3+. (e) Temperature-dependent fluorescence decay time constants of NIMO:10%Eu3+ and NIMO:40%Eu3+. (f) Temperature-dependent spontaneous decay rates of NIMO:10%Eu3+ and NIMO:40%Eu3+. | |
To further reveal the temperature quenching of the emission intensity in such materials, the dynamics of the 5D0–7FJ transition in NIMO:10%Eu3+ and NIMO:40%Eu3+ as a function of temperature are determined and shown in Fig. 5(d), which shows a regular change with increasing temperature. Based on the multi-phonon-relaxation theory, the total spontaneous emission rate of 5D0 can be written as follows:45
|
WT = WR + WNR(0) × (1 − exp(ℏω/kT))−ΔE/ℏω
| (4) |
WT represents the total spontaneous emission rate, WR represents the radiative transition rate, and WNR(0) represents the non-radiative transition rate at 0 K. By fitting, it is deduced that WR = 0.00273 ms−1 and WNR(0) = 41.5 ms−1 for NIMO:10% Eu3+, WR = 0.00274 ms−1 and WNR(0) = 31.4 ms−1 for NIMO:40%Eu3+. It can be seen that WR remain constant between NIMO:10%Eu3+ and NIMO:40%Eu3+, however, WNR(0) reduces by approximately 25% with increasing Eu3+ doping concentrations. This experiment results further indicate that the increase in the average spacing of Eu3+ by lattice interface barriers can effectively suppress non-radiative energy loss, as described in the above section.
3.4 Applications in red and warm white LEDs
The luminescence intensity of Eu3+ doped red phosphors is crucial for supplementing the red light component in commercial fluorescent powder. A red-emitting LED device is packaged by combining a 395 nm near-UV chip and the NIMO:90%Eu3+ phosphors in Fig. 6(a). The device emits bright red light visible to the naked eye (inset of Fig. 6(a)) and shows high color purity of 96%, representing its potential application in improving the color rendering performance of lighting devices. To confirm its practical application in warm white indoor lighting, a white LED device is encapsulated by combining the commercial BAM:Eu2+ blue phosphors, YAG:Ce3+ yellow phosphors and the as-prepared NIMO:90%Eu3+ onto the 395 nm near-UV chip in Fig. 6(a). As wishes, the coated white LED displays a bright white light emitting with slightly yellow (the lower part of Fig. 6(a), inset). The fabricated white LED shows an effective lighting performance with CIE chromaticity coordinates of (0.343, 0.335) (Fig. 6(b)), CRI of 92.1, CCT of 5013 K, color realism of 86.9, and color saturation of 101.1. All the experimental results indicates that the two-phase mixing NIMO:xEu3+ materials have potential application prospects in warm white LEDs.
|
| Fig. 6 (a) Electroluminescence performance of the fabricated red and white LED devices, the insets show their working conditions. (b) Corresponding chromaticity coordinates in the CIE diagram. | |
4. Conclusions
In summary, a series of highly efficient NIMO:xEu3+ (x = 10–90%) red light phosphors are successfully synthesized using a high-temperature solid-state method and concentration quenching inhibition is found in this system. The crystal structure, PLE and PL spectra, fluorescent dynamics and temperature-dependent luminescence properties are performed to comprehensively investigate its concentration quenching mechanism. As the Eu3+ doping concentration increases, the coexistence of Eu six-coordinated and eight-coordinated phases appears in the as-prepared materials. The increase lattice interface barriers can enlarge the average spacing of Eu in material, effectively suppress their CET, and enhance the red emission. The fluorescence lifetime does not change with the of Eu3+ doping concentration, indicating that the increase of CET in Eu six-coordination units and the decrease of CET by lattice interfaces barriers are mutually constrained. Temperature-dependent luminescence performance analysis shows that due to the regulatory effect of lattice interface barriers, the NIMO:40%Eu3+ sample has better luminescence thermal stability, and the non-radiative transition rate is suppressed by 25% compared to the NIMO:10%Eu3+. Finally, the encapsulated device displays an effective warm white light performance with suitable CIE coordinates of (0.343, 0.335), low CCT of 5013 K, and high CRI of 92.7. In brief, the experimental results show a new mechanism for regulating CET relationships in the two-phase mixing materials, and lays an important foundation for exploration and preparation of new and efficient luminescent materials for warm white LEDs.
Conflicts of interest
There are no conflicts to declare.
Acknowledgements
This work is financially supported by grants from the National Natural Science Foundation of China (No. 52102194); Key Research Projects of Colleges and Universities in Henan Province (No. 21A430027); Guangdong Basic and Applied Basic Research Foundation (No. 2021A1515010449); Interdisciplinary Sciences Project, Nanyang Institute of Technology.
References
- Y.-C. Lin, M. Karlsson and M. Bettinelli, Inorganic phosphor materials for lighting, Top. Curr. Chem., 2017, 374, 309–355 Search PubMed.
- V. Singh, P. Rohilla, S. Kaur and A. S. Rao, Tb3+ activated Na3YSi2O7 phosphors for display panels, Optik, 2022, 271, 170221 CrossRef CAS.
- D. L. Wei, H. J. Seo, Y. S. Liu and X. F. Yang, Broadband infrared emission of Pr3+-doped BiLa2O4.5 phosphor for optical amplifier applications, J. Lumin., 2023, 253, 119488 CrossRef CAS.
- X. J. Liu, T. Q. Chen, Y. Y. Gong, C. Li, L. Y. Niu, S. Q. Xu, X. T. Xu, L. K. Pan, J. G. Shapter, Y. Yamauchi, J. Na and M. Eguchi, Light-conversion phosphor nanoarchitectonics for improved light harvesting in sensitized solar cells, J. Photochem. Photobiol., C, 2021, 47, 100404 CrossRef CAS.
- J. M. Huang, P. F. Jiang, Z. Cheng, R. Wang, R. H. Cong and T. Yang, Structural confinement-induced highly efficient deep-red emission and negative thermal quenching performance in Mn4+-activated Ca7Mg2Ga6-yAlyO18:Mn4+ phosphors, Inorg. Chem. Front., 2023, 10, 2776–2787 RSC.
- L. Pu, Y. Wang, J. Zhao, M. Jin, L. Li, P. Li, Z. Wang, C. Guo and H. Suo, Multi-mode ratiometric thermometry using thermo-intensified NIR emission, Chem. Eng. J., 2022, 449, 137890 CrossRef CAS.
- F. Y. Zhao, Z. Song and Q. L. Liu, Advances in chromium-activated phosphors for near-infrared light sources, Laser Photonics Rev., 2022, 16, 2200380 CrossRef CAS.
- Q. Zhang, Y. Shi, D. Kosyanov, Y. Xiong, T. Wu, Z. Zhou, Q. Liu, J. Fang, J. Ni, H. He, J. Yu, M. Niu and W. Liu, Effect of extra added Mg2+ and Si4+ on the microstructure and luminescence properties of Ce:YAG ceramic phosphors for high power LED/LD lighting, Ceram. Int., 2023, 49, 11311–11322 CrossRef CAS.
- R. Zhang, H. Lin, Y. L. Yu, D. Q. Chen, J. Xu and Y. S. Wang, A new-generation color converter for high-power white LED: transparent Ce3+:YAG phosphor-in-glass, Laser Photonics Rev., 2014, 8, 158–164 CrossRef CAS.
- Q. Yao, P. Hu, P. Sun, M. Liu, R. Dong, K. Chao, Y. Liu, J. Jiang and H. Jiang, YAG:Ce3+ transparent ceramic phosphors brighten the next-generation laser-driven lighting, Adv. Mater., 2020, 32, 1907888 CrossRef CAS PubMed.
- D. Q. Chen, Y. Zhou and J. S. Zhong, A review on Mn4+ activators in solids for warm white light-emitting diodes, RSC Adv., 2016, 6, 86285–86296 RSC.
- L. Huang, Y. Zhu, X. Zhang, R. Zou, F. Pan, J. Wang and M. Wu, Hf-free hydrothermal route for synthesis of highly efficient narrow-band red emitting phosphor K2Si1-xF6:xMn4+ for warm white light-emitting diodes, Chem. Mater., 2016, 28, 1495–1502 CrossRef CAS.
- C. Y. Jiang, L. H. Li, M. G. Brik, L. T. Lin and M. Y. Peng, Epitaxial growth via anti-solvent-induced deposition towards a highly efficient and stable Mn4+ doped fluoride red phosphor for application in warm WLEDs, J. Mater. Chem. C, 2019, 7, 6077–6084 RSC.
- X. Huang, B. Li, H. Guo and D. Chen, Molybdenum-doping-induced photoluminescence enhancement in Eu3+-activated CaWO4 red-emitting phosphors for white light-emitting diodes, Dyes Pigm., 2017, 143, 86–94 CrossRef CAS.
- R. Nagaraj, A. Raja and S. Ranjith, Synthesis and luminescence properties of novel red-emitting Eu3+ ions doped silicate phosphors for photonic applications, J. Alloys Compd., 2020, 827, 154287 CrossRef.
- Q. Wu, Y. Xie, F. She, Q. Zhao, J. Ding and J. Zhou, CsBaB3O6:Eu3+ red-emitting phosphors for white LED and FED: crystal structure, electronic structure and luminescent properties, J. Rare Earths, 2021, 39, 1040–1048 CrossRef CAS.
- T. Gavrilovic, J. Perisa, Z. Ristic, K. Elzbieciak-Piecka, L. Marciniak, C.-G. Ma, Z. Antic and M. D. Dramicanin, Thermal history forensics using the emission intensity ratio of YVO4: Eu3+ phosphor, Measurement, 2022, 202, 111942 CrossRef.
- B. Yu, Y. Li, Y. Wang and L. Geng, Double-site Eu3+ occupation in the langbeinite-type phosphate phosphor toward adjustable emission for pc-WLEDs, J. Alloys Compd., 2021, 874, 159862 CrossRef CAS.
- K. Thomas, D. Alexander, K. P. Mani, S. Gopi, S. A. Kumar, P. R. Biju, N. V. Unnikrishnan and C. Joseph, Intrinsic red luminescence of Eu3+-activated lanthanum molybdate: insights into the spectroscopic features using Judd-Ofelt theoretical analysis, J. Phys. Chem. Solids, 2020, 137, 109212 CrossRef CAS.
- Y. Zhang, X. Zhu, Y. Zhao, Q. Zhang, Q. Dai, L. Lu and L. Zhang, CdWO4:Eu3+ Nanostructures for Luminescent Applications, ACS Appl. Nano Mater., 2019, 2, 7095–7102 CrossRef CAS.
- Y. Liu, J. Li, H. Zuo, X. Shi, S. Ma and M. Zhao, Synthesis and luminescent properties of KLa1-x-y(MoO4)2-z(WO4)z:xEu3+, yDy3+ phosphors for WLEDs, J. Mater. Sci.: Mater. Electron., 2016, 27, 9470–9475 CrossRef CAS.
- Q. Cheng, F. Ren, Q. Lin, H. Tong and X. Miao, High quantum efficiency red emitting alpha-phase La2W2O9:Eu3+ phosphor, J. Alloys Compd., 2019, 772, 905–911 CrossRef CAS.
- J. Afshani, T. Delgado, G. Paveliuc and H. Hagemann, Luminescence spectroscopy of CaAl12O19:Eu3+ and SrAl12O19: Eu3+ nanoparticles, J. Lumin., 2022, 246, 118805 CrossRef CAS.
- A. I. Becerro, M. Allix, M. Laguna, D. Gonzalez-Mancebo, C. Genevois, A. Caballero, G. Lozano, N. O. Nunez and M. Ocana, Revealing the substitution mechanism in Eu3+:CaMoO4 and Eu3+,Na+:CaMoO4 phosphors, J. Mater. Chem. C, 2018, 6, 12830–12840 RSC.
- X. Qiao, J. Xin, X. Nie, J. Xu, S. Qi and Z. Jiang, The structure-dependent luminescence of Eu3+-activated MBaY(BO3)2 (M=Na, K) nanoparticles, Dyes Pigm., 2017, 143, 103–111 CrossRef CAS.
- S. Wang, Y. Xu, T. Chen, W. Jiang, J. Liu, X. Zhang, W. Jiang and L. Wang, A red phosphor LaSc3(BO3)4:Eu3+ with zero-thermal-quenching and high quantum efficiency for LEDs, Chem. Eng. J., 2021, 404, 125912 CrossRef CAS.
- N. Yang, J. Li, Z. Zhang, D. Wen, Q. Liang, J. Zhou, J. Yan and J. Shi, Delayed concentration quenching of luminescence caused by Eu3+-induced phase transition in LaSc3(BO3)4, Chem. Mater., 2020, 32, 6958–6967 CrossRef CAS.
- K. Singh, M. Rajendran, R. Devi and S. Vaidyanathan, Narrow-band red-emitting phosphor with negligible concentration quenching for hybrid white LEDs and plant growth applications, Dalton Trans., 2021, 50, 4986–5000 RSC.
- S. Priyansha, J. Madda and S. Vaidyanathan, Narrow band dazzling red emitting (LiCaLa(MoO4)3:Eu3+) phosphor with scheelite structure for hybrid white LEDs and LiCaLa(MoO4)3:Sm3+, Eu3+ based deep-red LEDs for plant growth applications, Dalton Trans., 2023 10.1039/D3DT02716C.
- J. Chen, X. F. Yang, C. Y. Jiang, Y. F. Wang, L. Zhou and M. M. Wu, Second-phase-induced fluorescence quenching in non-equivalent substituted red phosphors, RSC Adv., 2022, 12, 29338–29345 RSC.
- M. Maczka, Vibrational characteristics of the alkali metal-indium double molybdates MIn(MoO4)2 and tungstates MIn(WO4)2 (M=Li, Na, K, Cs), Int. J. Quantum Chem., 1997, 129, 287–297 CAS.
- J. P. Li, G. L. Mo, Y. H. Bai and A. Bao, Microwave-assistant hydrothermal synthesis and luminescence of NaEu(MoO4)2:Sm3+ powders, J. Mater. Sci.: Mater. Electron., 2015, 26, 7390–7396 CrossRef CAS.
- C. G. Yang, Y. G. Liu, H. J. Yu, Y. K. Liu, J. Y. Yang, C. A. Xie, L. L. Wang and R. Y. Mi, Using energy transfer to obtain warm white-emitting and thermally stable Ca3Y(AlO)3(BO3)4:Dy3+, Eu3+ phosphors, J. Lumin., 2023, 260, 119875 CrossRef CAS.
- V. Sivakumar and U. V. Varadaraju, Intense red-emitting phosphors for white light emitting diodes, J. Electrochem. Soc., 2005, 152, H168 CrossRef CAS.
- F. M. Emen and R. Altinkaya, Luminescence and thermoluminescence properties of Sr3WO6:Eu3+ phosphor, J. Lumin., 2013, 134, 618–621 CrossRef CAS.
- R. Phatak, N. Pathak, S. Muhammed, S. K. Sali and A. Das, Crystal structure and site symmetry of undoped and Eu3+ doped Ba2LaSbO6 and BaLaMSbO6 compounds (M= Mg, Ca): tuning europium site occupancy to develop orange and red phosphor, ChemPlusChem, 2018, 83, 1144–1152 CrossRef CAS PubMed.
- N. Pathak, S. Mukherjee, B. P. Mandal, A. K. Yadav, S. N. Jha and D. Bhattacharyya, Interplay between local distortion at lattice sites with optical and electrical properties of Eu3+-doped MNbO3 (M= Na and K) compounds, Mater. Adv., 2020, 1, 2380–2394 RSC.
- X. Huang, S. Wang, B. Li, Q. Sun and H. Guo, High-brightness and high-color purity red-emitting Ca3Lu(AlO)3(BO3)4:Eu3+ phosphors with internal quantum efficiency close to unity for near-ultraviolet-based white-light-emitting diodes, Opt. Lett., 2018, 43, 1307–1310 CrossRef CAS PubMed.
- P. P. Dang, G. G. Li, X. H. Yun, Q. Q. Zhang, D. J. Liu, H. Z. Lian, M. M. Shang and J. Lin, Thermally stable and highly efficient red-emitting Eu3+-doped Cs3GdGe3O9 phosphors for WLEDs: non-concentration quenching and negative thermal expansion, Light: Sci. Appl., 2021, 10, 29 CrossRef CAS PubMed.
- G. Blasse, Energy transfer between inequivalent Eu2+ ions, J. Solid State Chem., 1986, 62, 207–211 CrossRef CAS.
- N. Pathak, S. Mukherjee, D. Das, D. Dutta, S. Dash and R. M. Kadam, Evolution of different defect clusters in Eu3+ doped KMgF3 and Eu3+, Li+ co-doped KMgF3 compounds and the immediate impact on the phosphor characteristics, J. Mater. Chem. C, 2020, 8, 7149–7161 RSC.
- S. Mukherjee, N. Pathak, D. Das and D. Dutta, Engineering defect clusters in distorted NaMgF3 perovskite and their important roles in tuning the emission characteristics of Eu3+ dopant ion, RSC Adv., 2021, 11, 5815–5831 RSC.
- Y. B. Hua, W. G. Ran and J. S. Yu, Excellent photoluminescence and cathodoluminescence properties in Eu3+-activated Sr2LaNbO6 materials for multifunctional applications, Chem. Eng. J., 2021, 406, 127154 CrossRef CAS.
- B. Li, X. Y. Huang, H. Guo and Y. J. Zeng, Energy transfer and tunable photoluminescence of LaBWO6:Tb3+,Eu3+ phosphors for near-UV white LEDs, Dyes Pigm., 2018, 150, 67–72 CrossRef CAS.
- Y. F. Wang, Y. S. Zhu, W. Xu, H. W. Song, S. Xu, J. Wang and H. N. Cui, Self assembly of three-dimensional Lu2O3:Eu3+ inverse opal photonic crystals, their modified emissions and dual-functional refractive index sensing, Dalton Trans., 2013, 42, 14014–14020 RSC.
|
This journal is © The Royal Society of Chemistry 2023 |
Click here to see how this site uses Cookies. View our privacy policy here.