Yoshihiro
Goto
*,
Kiyoshi
Yamazaki
*,
Masashi
Kikugawa
and
Masakazu
Aoki
Toyota Central R&D Labs., Inc., 41-1 Yokomichi, Nagakute, Aichi 480-1192, Japan. E-mail: yoshihiro-goto@mosk.tytlabs.co.jp; e0936@mosk.tytlabs.co.jp
First published on 7th August 2024
The reverse water–gas shift chemical looping (RWGS-CL) process that utilizes redox reactions of metal oxides is promising for converting CO2 to CO at low temperatures. Metal oxides with perovskite structures, particularly, perovskite LaCoO3 are promising frameworks for designing RWGS-CL materials as they can often release oxygen atoms topotactically to form oxygen vacancies. In this study, solid solutions of perovskite LaCo1−xAlxO3 (0 ≤ x ≤ 1), which exhibited high CO production capability and thermal stability under the RWGS-CL process, were developed. Al-substituted LaCo0.5Al0.5O3 (x = 0.5) exhibited a 4.1 times higher CO production rate (2.97 × 10−4 CO mol g−1 min−1) than that of LaCoO3 (x = 0; 0.73 × 10−4 CO mol g−1 min−1). Diffuse reflectance infrared Fourier transform spectroscopy studies suggested that an increase in CO2 adsorption sites produced by the coexistence of Al and Co was responsible for the enhancement of CO production rate. Furthermore, LaCo0.5Al0.5O3 maintained its perovskite structure during the RWGS-CL process at 500 °C without significant decomposition, whereas LaCoO3 decomposed into La2O3 and Co0. In situ X-ray diffraction study revealed that the high thermal stability was attributed to the suppression of phase transition into a brownmillerite structure with ordered oxygen vacancies. These findings provide a critical design approach for the industrial application of perovskite oxides in the RWGS-CL processes.
A possible first step in utilizing captured CO2 is to convert it into carbon monoxide (CO), which serves as a crucial raw material for synthetic fuels and various chemical products.8 This conversion is generally carried out by a catalytic reverse water–gas shift reaction (RWGS reaction; CO2 + H2 → CO + H2O), which requires high temperature due to thermodynamic constraints.9 For example, temperatures greater than 750 °C are required to achieve a CO2 conversion of 80%. To decrease this operating temperature, the RWGS chemical looping (RWGS-CL) process using metal oxides has been actively investigated in recent years.10 The RWGS-CL process consists of sequential reactions of reduction (MOx + δH2 → MOx−δ + δH2O) and re-oxidation (MOx−δ + δCO2 → MOx + δCO) of metal oxides. In contrast to catalytic RWGS reaction, which uses a mixture of H2 and CO2 in a certain ratio, the RWGS-CL process is not limited by thermodynamic constraints because the reduction and the oxidation processes are separate, exhibiting the potential for high CO2 conversion even at low temperatures (<500 °C).11 Moreover, continuous CO production is achieved by using a fixed bed system in which H2 and CO2 are alternately provided to two reactors filled with metal oxides (Fig. 1a) or a circulating fluidized bed system (Fig. 1b) in which the metal oxides are circulated between the oxidation and the reduction reactors.12
Fig. 1 CO production flowchart based on reverse water–gas shift reaction chemical looping (RWGS-CL) process using (a) periodically operated fixed bed system and (b) circulating fluidized bed system. |
These systems do not require a water separation process for the produced CO and do not generate methane as a common by-product, resulting in the RWGS-CL process demonstrating higher energy efficiency than the catalytic RWGS reaction.13
The performance of the RWGS-CL process is substantially affected by the metal oxides that are responsible for the reduction and re-oxidation reactions. Metal oxides, where some transition metals (e.g., Mn, Fe, Co, and Ni)14–17 and some triels (In and Ga)11,18 act as redox species, have been reported as materials for the RWGS-CL process (RWGS-CL materials). To produce CO in the oxidation process with CO2, RWGS-CL materials are required to form a large number of oxygen vacancies, which work as active sites for CO2 conversion, in the reduction process with H2.19 Metal oxides with perovskite structures can often release oxygen atoms topotactically to form oxygen vacancies; hence, they are promising frameworks for designing RWGS-CL materials. In particular, perovskite LaCoO3, which demonstrates catalytic RWGS reaction activity,20 is capable of stabilizing a large number of oxygen vacancies.21 However, LaCoO3 is not suitable for the RWGS-CL process because of its poor thermal stability in a reducing atmosphere (decomposition starts at 500 °C).22 We recently demonstrated that the thermal stability of perovskite LaNiO3 can be enhanced by Al substitution of a Ni site.23 In this study, we attempted Al substitution of a Co site in perovskite LaCoO3 and investigated the effects of Al substitution on thermal stability in a reducing atmosphere and RWGS-CL performance. Al substitution enhanced the thermal stability and prevented phase decomposition at a typical operating temperature of 500 °C during the RWGS-CL process. Notably, although the number of oxygen vacancies formed in LaCo1−xAlxO3 decreased with increasing Al substitution, the CO production rate increased. LaCo0.5Al0.5O3 did not exhibit any degradation after 32 cycles of the RWGS-CL stability test, indicating that LaCo1−xAlxO3 has potential as a RWGS-CL material.
X-ray diffraction (XRD) patterns of the samples were collected using an Ultima IV X-ray diffractometer (Rigaku) with Cu Kα radiation (λ = 1.54056 Å). The XRD patterns were obtained in the range 2θ = 20°–80° in steps of 0.01° at room temperature. In situ synchrotron X-ray diffraction (SXRD) patterns of the samples were obtained using a Debye–Scherrer camera with a two-dimensional detector (PILATUS 100 K) installed in the BL5S2 beamline at the Aichi Synchrotron Radiation Center. The quartz glass capillaries (0.3 mm o.d.) filled with the samples were irradiated with X-rays at a wavelength of λ = 0.689826 Å. The atmosphere in the capillaries was either air or 100% H2. Both patterns were obtained at either room temperature or 500 °C. The collected XRD and in situ SXRD patterns were analyzed using the Le Bail method implemented in JANA2006.24 Diffuse reflectance infrared Fourier transform (DRIFT) spectra of samples were recorded at 500 °C under a flow of 5% CO2/N2 (200 mL min−1) using an iS50 spectrometer (Thermo Fisher). These samples (40 mg) were preheated at 500 °C for 30 min under a flow of 5% H2/N2 (200 mL min−1). Thermogravimetric analysis (TGA) was conducted using a thermogravimeter analyzer (TGA-50, Shimadzu) connected to mass flow controllers. The temperature dependence of the TGA curves of the samples (20 mg) was recorded up to 800 °C at a ramp rate of 10 °C min−1 under a flow of 5% H2/N2 (100 mL min−1). The RWGS-CL performance of the samples (20 mg) was evaluated from the isothermal TGA curves recorded upon switching between a flow of 5% H2/N2 (100 mL min−1) and 5% CO2/N2 (100 mL min−1) every 30 min at 200–500 °C. The CO production rate was estimated from the weight loss during the initial 30 s under 5% H2/N2. The amount of CO produced was estimated from the total weight loss after 30 min under a 5% H2/N2 flow. CO production was also confirmed by additional experiments using a fixed bed reactor, in which the reaction gas can be analyzed by mass spectrometry (infiTOF, KANOMAX JAPAN) or Fourier-transform infrared (FT-IR) spectroscopy (Bex-100FT, Best-Sokki).
Fig. 2 (a) X-ray diffraction (XRD) patterns of LaCo1−xAlxO3 (0 ≤ x ≤ 1). (b) Lattice volumes of LaCo1−xAlxO3 as a function of Al content (x). |
The oxygen release behavior of LaCo1−xAlxO3 is investigated using TGA, recorded upon heating to 800 °C under a flow of 5% H2/N2 (Fig. 3). The TGA curve of LaAlO3 (x = 1) did not exhibit any weight loss upon heating to 800 °C, whereas all the TGA curves of Co-containing LaCo1−xAlxO3 (x = 0, 0.25, 0.5, 0.75) exhibited weight losses at 300–500 °C, indicating that these weight losses were attributed to the oxygen release associated with the reduction of Co3+. The amount of weight loss up to 500 °C decreased with an increase in the Al content because of the decrease in the Co content. These weight losses correspond to the reduction of Co3+ to Co2.04–2.11+. All XRD patterns of LaCo1−xAlxO3 quenched at 500 °C in the TGA measurements are indexed by their original rhombohedral perovskite structure (space group: Rc) without any separated phase (Fig. S1†). These observations suggest that Co-containing LaCo1−xAlxO3 (Co3+) transform into LaCo1−xAlxO3−δ (Co2+; δ = (1−x)/2) following topotactic oxygen release from their crystal lattices.
Fig. 3 Thermogravimetric analysis curves of LaCo1−xAlxO3 (0 ≤ x ≤ 1) during heating in the flow of 5% H2/N2. Black arrows indicate the onset temperature of decomposition. |
The TGA curve of LaCoO3 (x = 0) exhibited further weight loss in the range 600–700 °C. The weight loss up to 700 °C (9.3 wt%) was 3.0 times higher than that observed up to 500 °C (3.1 wt%), suggesting the sequential reduction of LaCoO3 (Co3+) into LaCoO2.5 (Co2+), followed by decomposition into Co (Co0) and La2O3. The Co and La2O3 phases are shown in the XRD pattern of LaCoO3 quenched at 800 °C in the TGA measurements (Fig. S2†), attributing the weight loss at 600–700 °C to phase decomposition. The phase decomposition temperature (black arrows in Fig. 3) increases with increasing Al content: 600, 660, and 670 °C for LaCoO3 (x = 0), LaCo0.75Al0.25O3 (x = 0.25), and LaCo0.5Al0.5O3 (x = 0.5), respectively. LaCo0.25Al0.75O3 (x = 0.75) and LaAlO3 (x = 1) did not exhibit any significant weight loss in the range 500–800 °C. The XRD patterns of the samples quenched at 800 °C reveal that undergoes LaCo0.75Al0.25O3 (x = 0.25) partial decomposition, while still maintaining the perovskite phase. LaCo0.5Al0.5O3 (x = 0.5), LaCo0.25Al0.75O3 (x = 0.75), and LaAlO3 (x = 1) does not show any phase decomposition (Fig. S2†). These results show that Al substitution enhances the structural stability of perovskite LaCo1−xAlxO3 in a reducing atmosphere.
In situ SXRD measurements were conducted to investigate the reasons for the enhanced structural stability. The SXRD patterns of LaCoO3 (x = 0) and LaCo0.5Al0.5O3 (x = 0.5) are indexed to a rhombohedral perovskite structure (space group: Rc) without any impurity phases at room temperature in air (Fig. 4). The estimated lattice volumes of LaCoO3 and LaCo0.5Al0.5O3 (V = 335.80(3) and 329.25(4) Å3, respectively, Fig. S3†) agreed with those estimated from the XRD patterns (Fig. 2). Heating these samples to 500 °C in air did not change their crystal structures. Peak shifts toward lower angles were observed for both samples, indicating an increase in the lattice volumes owing to thermal expansions.29 The lattice volumes of LaCoO3 and LaCo0.5Al0.5O3 at 500 °C were V = 347.80(6) and 336.62(5) Å3, respectively (Fig. S3†), corresponding to thermal expansions of 3.6% and 2.2%, respectively, relative to those at room temperature. The SXRD pattern of LaCoO3 obtained 5 min after switching the atmosphere from air to H2 at 500 °C is characterized by an orthorhombic brownmillerite structure with a space group of Pnma and a small amount of La2O3 (Fig. 4a). The brownmillerite structure was identical to the reported structure of LaCoO2.5 (La2Co2O5), which was produced by the reduction of LaCoO3.30 The brownmillerite phase observed in the SXRD pattern was identified as LaCoO2.5. This determination was based on the estimated composition of LaCoO3, which was found to be reduced at 500 °C in the TGA analysis (LaCoO2.52), resulting in a composition similar to that of LaCoO2.5. The peak intensities of the brownmillerite phase decreased 30 min after atmospheric switching, whereas those of La2O3 increased simultaneously. An additional Co metal phase was observed. These observations show that brownmillerite LaCoO2.5, which is formed by the reduction of perovskite LaCoO3, gradually decomposes into Co and La2O3 under a reducing atmosphere at 500 °C (Fig. 5). In contrast, the SXRD pattern of LaCo0.5Al0.5O3 shows that the perovskite phase maintained its original rhombohedral perovskite structure 30 min after switching the atmosphere from air to H2 at 500 °C (Fig. 4b). No phase decomposition was observed. Moreover, LaCoO3 and LaCo0.5Al0.5O3 exhibited an increase in the lattice volumes after switching the atmosphere from air to H2 at 500 °C (Fig. S3†). This finding could be attributed to an increase in the ionic radius of Co from 0.61 Å (Co3+) to 0.745 Å (Co2+) owing to the reduction of LaCoO3 and LaCo0.5Al0.5O3. Therefore, in situ SXRD measurements suggest that the suppression of phase transition from the perovskite to the brownmillerite structure in a reducing atmosphere is responsible for the enhancement of the structural stability.
Fig. 4 In situ synchrotron XRD patterns of (a) LaCoO3 and (b) LaCo0.5Al0.5O3 collected at room temperature in air, 500 °C in air, and 500 °C in 100% H2 (5 and 30 min). |
Fig. 5 Schematic of the structural changes in (a) LaCoO3 and (b) LaCo0.5Al0.5O3 at 500 °C. White, blue, green, and red spheres represent La, Co, Al, and O, respectively. The crystal structures were depicted by VESTA program.31 |
The effect of crystallographic differences on structural stability is often explained by the coordination number (CN) of redox species.23,32 In perovskite LaNi1−xAlxO3, suppression of the formation of Ni2+ with small CN (four-coordinated NiO4) in a reducing atmosphere prevents further reduction to Ni0+, leading to phase decomposition.23 All Co atoms in the crystal lattice of LaCoO3 and LaCo0.5Al0.5O3 form CoO6 octahedra (CN = 6) in an oxidizing atmosphere (Fig. 5). The brownmillerite LaCoO2.5, observed for LaCoO3 in a reducing atmosphere, has a vacancy-ordered structure comprising original CoO6 octahedra and CoO4 tetrahedra (CN = 4), where two O atoms are removed from the CoO6 octahedra. Evidently, two oxygen atoms were removed from two neighboring octahedra in the perovskite structure; the formation of one tetrahedron that can form a vacancy-ordered structure is energetically more stable than the formation of two pentahedral (CN = 5).33 In contrast, LaCo0.5Al0.5O3 maintained its original rhombohedral perovskite structure in a reducing atmosphere, indicating that CoO5 pentahedra rather than CoO4 tetrahedra were predominantly formed by the reduction of LaCo0.5Al0.5O3. This finding could be attributed to the random substitution of irreducible Al in LaCo0.5Al0.5O3, which reduces the number of neighboring CoO6 octahedra, preventing oxygen vacancy ordering resulting in the formation of CoO4 tetrahedra. Suppression of the formation of CoO4 tetrahedra with less CN enhanced the structural stability of LaCo0.5Al0.5O3 in a reducing atmosphere.
The RWGS-CL performance of LaCo1−xAlxO3 is evaluated from the weight change upon alternately switching the atmosphere between 5% H2/N2 and CO2/N2 every 30 min at an isothermal temperature of 500 °C (Fig. 6a). Co-containing LaCo1−xAlxO3 (x = 0, 0.25, 0.5, and 0.75) exhibited weight losses in the initial 5% H2/N2 atmosphere (0–30 min) attributed to the oxygen release associated with Co3+ reduction. The amount of weight loss decreased with increasing Al content, indicating a decrease in the number of oxygen vacancies formed. The weights of the samples increased again when the atmosphere was switched to 5% CO2/N2 (30–60 min). The increase in weight was derived from oxygen intake associated with the oxidation of Co2+, which resulted in the formation of CO through the reduction of CO2. CO production was also confirmed by mass spectrometry (Fig. S4†) and FT-IR spectroscopy (Fig. S5†). Although these methods can quantify the CO production amount, they are not suitable for quantifying the CO production rate because of the effect of gas diffusion. Thus, CO production is often estimated from weight changes.11,18 When the atmosphere was subsequently switched again to 5% H2/N2 (60–90 min), the weight of LaCo1−xAlxO3 (x = 0.25, 0.5, and 0.75) decreased to the same weight as that in the initial 5% H2/N2 atmosphere (0–30 min), whereas the weight of LaCoO3 (x = 0) decreased more than that in the initial 5% H2/N2 atmosphere (0–30 min). The RWGS-CL profiles normalized by the fraction of reduced Co3+ ([Co2+]/([Co2+] + [Co3+])) show that the fraction of LaCo1−xAlxO3 (x = 0.25, 0.5, and 0.75) becomes constant at approximately 100% in 5% H2/N2, whereas that of LaCoO3 exceeds 100% (Fig. S6†). This finding suggests that Co3+ in LaCo1−xAlxO3 (x = 0.25, 0.5, and 0.75) is stabilized by Co2+ in a reducing atmosphere, whereas Co3+ in LaCoO3 is not stabilized by Co2+ and is further reduced. The XRD patterns of samples after the RWGS-CL reaction (Fig. S7†) reveal that only LaCoO3 contained La2O3 in addition to its original perovskite phase, indicating that the reduction of Co2+ is accompanied by a phase separation, which is consistent with the fact that LaCoO3 gradually decomposes into Co and La2O3 in a reducing atmosphere, as revealed by the in situ SXRD experiment (Fig. 5). Therefore, the RWGS-CL reaction of LaCo1−xAlxO3 (x = 0.25, 0.5, and 0.75) containing Co and Al corresponds to the following topotactic redox reactions:
LaCo1−xAlxO3 + δH2 → LaCo1−xAlxO3−δ + δH2O | (1) |
LaCo1−xAlxO3−δ + δCO2 → LaCo1−xAlxO3 + δCO | (2) |
The CO production rate per unit mass (CO mol g−1 min−1), which is estimated from the weight change rate in 5% CO2/N2 at 500 °C, is maximum at x = 0.5–0.75 for LaCo1−xAlxO3 (Fig. 6b). For example, the CO production rate of LaCo0.5Al0.5O3 (x = 0.5; 2.97 × 10−4 CO mol g−1 min−1) was 4.1 times higher than that of LaCoO3 (x = 0; 0.73 × 10−4 CO mol g−1 min−1). The higher CO production rate per unit mass despite the lower Co content is derived from the fact that the CO production rate per Co atom (CO mol−1 min−1) increased with increasing Al content (Fig. 6b: 0 ≤ x ≤ 0.75). The DRIFT spectra of LaCoO3 (x = 0) and LaCo0.75Al0.25O3 (x = 0.25) in 5% CO2/N2 at 500 °C (Fig. S8†) exhibited only one absorption peak at approximately 2350 cm−1, corresponding to the CO2 gas phase,34 whereas that of LaCo0.5Al0.5O3 (x = 0.5) exhibited additional broad peaks at 1252 and 1529 cm−1 derived from carbonate (CO32−).35 However, the adsorption modes of carbonate could not be identified because of the broadness of the peaks. The oxygen atoms required for carbonate formation can come from LaCo1−xAlxO3−δ itself or supplied to LaCo1−xAlxO3−δ during the RWGS-CL reaction in eqn (2). LaCo0.25Al0.75O3 (x = 0.75) had larger peaks at 1186 and 1685 cm−1, originating from carbonates; however, LaAlO3 (x = 1) did not exhibit any peaks associated with carbonates. The results of the DRIFT experiments suggest that the coexistence of a suitable amount of Al and Co (0.5 ≤ x ≤ 0.75) in LaCo1−xAlxO3 increases the CO2 adsorption sites. The increased number of CO2 adsorption sites promotes CO2 dissociation at an oxygen vacancy as an active site, which in turn enhances the CO production rate.
The CO production amount per unit mass (CO mol g−1) at 500 °C is maximum at x = 0.5 (LaCo0.5Al0.5O3; 4.67 × 10−4 CO mol g−1) for LaCo1−xAlxO3 (Fig. 6c). The amount of CO produced per Co atom (CO mol−1) increased with an increase in the Al content (0 ≤ x ≤ 0.75) owing to the increase in the CO production rate. A trade-off between the increase in the CO production amount per Co atom and decrease in Co content would result in the maximum CO production amount per unit mass at x = 0.5. Additionally, the temperature dependence of the CO production amount per unit mass in the RWGS-CL reaction was investigated (Fig. S10†). LaCo1−xAlxO3 (x = 0, 0.25, 0.5, 0.75, and 1) showed almost no CO production at 200 °C, whereas Co-containing LaCo1−xAlxO3 (x = 0, 0.25, 0.5, and 0.75) produced CO at ≥300 °C. Interestingly, Al-substituted LaCo1−xAlxO3 (x = 0.25, 0.5, and 0.75) produced more CO than LaCoO3 (x = 0) at ≥400 °C, indicating the effect of the coexistence of Al and Co. Moreover, the amount of CO producing LaCo0.5Al0.5O3 exhibits no degradation over 32 cycles of the RWGS-CL stability test at 500 °C (Fig. S9†), demonstrating that LaCo0.5Al0.5O3 is usable as a practical RWGS-CL material.
The RWGS-CL performance of LaCo0.5Al0.5O3 was then compared with those of perovskite La0.6Ca0.4Fe0.4Mn0.6O3 (LCFMO)14 and Co/In2O3,11 which have been reported to exhibit high CO2 conversion activity and stability. The order of the CO production rate at 500 °C is LCFMO > LaCo0.5Al0.5O3 > Co/In2O3, which possibly reflects the order of the number of CO2 adsorption sites or the activity of oxygen vacancies (Fig. S11a†). The CO production amount of Co/In2O3 (1.90 × 10−3 CO mol g−1) is 4.0 and 3.3 times higher than that of LaCo0.5Al0.5O3 (0.47 × 10−3 CO mol g−1) and LCFMO (0.58 × 10−3 CO mol g−1), respectively (Fig. S11b†). This finding is attributed to the fact that the theoretical maximum CO production amount estimated from the content of redox species in Co/In2O3 (In3+ ↔ In0: 17.8 mmol g−1) was 8.2 and 3.6 times higher than that of LaCo0.5Al0.5O3 (Co3+ ↔ Co2+: 2.18 mmol g−1) and LCFMO (Fe3+ ↔ Fe2+ and Fe4+ ↔ Fe3+: 4.93 mmol g−1), respectively. Notably, the oxygen release rate, an indicator of regeneration rate of samples in H2 atmosphere, of LaCo0.5Al0.5O3 (6.02 × 10−4 O mol g−1 min−1) is 6.4 and 4.7 times higher than that of LCFMO (0.94 × 10−4 O mol g−1 min−1) and Co/In2O3 (1.27 × 10−4 O mol g−1 min−1), respectively (Fig. S11c†). The oxygen release reaction in Co/In2O3 is associated with the formation of Co–In alloys from Co and In2O3,11 whereas that in LaCo0.5Al0.5O3 is accompanied by a topotactic reaction (eqn (1): from LaCo0.5Al0.5O3 to LaCo0.5Al0.5O2.75), which does not change the basic crystal structure. The relatively low energy required for oxygen release by the topotactic reaction may explain the higher oxygen release rate of LaCo0.5Al0.5O3 than that of Co/In2O3. Moreover, the higher oxygen release rate of LaCo0.5Al0.5O3 over that of LCFMO could be attributed to the fact that Co3+ is more readily reduced than Fe3+ and Mn4+.36 The RWGS-CL reaction system is expected to conduct reduction and oxidation reactions in parallel (Fig. 1); hence, RWGS-CL materials are required to exhibit high oxygen release and CO production rates. Therefore, LaCo0.5Al0.5O3, with a high oxygen release rate in addition to a high CO production rate, is a suitable material for the RWGS-CL process.
Footnote |
† Electronic supplementary information (ESI) available: Experimental details, XRD patterns, lattice volumes, mass spectra, CO concentration, isothermal RWGS-CL profiles, DRIFT spectra, and various RWGS-CL performances. See DOI: https://doi.org/10.1039/d4dt01743a |
This journal is © The Royal Society of Chemistry 2024 |