Neha
Saini
,
Kirti
Dhingra
,
Amit
Kumar
and
Kamalakannan
Kailasam
*
Institute of Nano Science and Nanotechnology, Knowledge city, Sector-81, Manauli, SAS Nagar, 140306 Mohali, Punjab, India. E-mail: kamal@inst.ac.in
First published on 11th September 2024
The utilization of mild and environment-friendly reaction conditions for the photocatalytic oxidation of sulfides to highly valuable sulfoxides represents a sustainable approach that is highly desirable yet quite challenging. Herein, we present a novel approach to enhance the photocatalytic oxidation of sulfides in water by molecular structural engineering of donor–acceptor (D–A) based polymeric networks. By incorporating electron-deficient heptazine or triazine units as acceptors and electron-rich 2,5-diamino fluorene as donors, a synergistic effect is achieved, promoting efficient charge separation upon light absorption. The two polymeric networks namely HEP-FL and TZ-FL efficiently carried out selective oxidation of sulfides to sulfoxide with 100% conversion within 1.3 h and 3.5 h, respectively under blue light irradiation. Through advanced spectroscopic and electrochemical measurements, the correlation between molecular structures and optoelectronic properties is elucidated, unveiling tunable band structures and exciton binding energies. Notably, the heptazine-containing polymeric network (HEP-FL) exhibited superior charge separation efficiency and enhanced catalytic activity, attributed to improved electron delocalization and reduced exciton binding energy. Additionally, we have performed green metrics calculations for the synthesis of sulfoxide using HEP-FL as a photocatalyst to prove the sustainability of the reaction system. These findings underscore the significant prospects of donor–acceptor-based polymeric networks as highly effective photocatalysts for selective oxidation reactions, highlighting their potential to advance environmentally conscious practices in organic synthesis and industrial applications.
The oxidation of sulfides to sulfoxides emerges as a compelling and consequential oxidation reaction, finding wide utility in organic synthesis and serving as active components in the pharmaceutical and agrochemical sectors.10–13 Many conventional methods for oxidizing sulfides to sulfoxides rely on oxidants such as m-CPBA, TBHP, UHP, IBX, or Oxone. These methods often involve excessive amounts of oxidants, catalysts, or high temperatures, leading to the formation of undesired byproducts. To mitigate these challenges and advance environmentally conscious practices, ongoing research endeavors focus on the development of novel catalysts and sustainable strategies.
In this regard, oxygen is considered a green and mild oxidant, which offers several advantages including its ambient nature, abundant availability, and harmlessness at ambient pressure.14,15 Consequently, the use of molecular oxygen as an oxidant can be considered the most environmentally conscious approach for oxidation reactions, aligning with the principles of sustainability and green chemistry. However, its activation is a challenging task due to the substantial kinetic barriers involved.
In the pursuit of efficient photocatalytic systems for sulfide oxidation to sulfoxides, inorganic photocatalytic materials like Bi4O5Br216 and Pt/BiVO417 have been investigated but face limitations such as low activity under visible light and poor selectivity. To address these issues, researchers have explored molecular coordination complexes, organic–inorganic hybrid18 photocatalysts (Table S1†), including dye-TiO2 assemblies,19 CdS/C3N4,20 metal–organic frameworks21,22 such as Zr6-Irphen,23 and composites like C60@PCN-222.24 However, most of these systems often require the incorporation of a crucial redox mediator like TEMPO.25,26 Despite these efforts, the photocatalytic activity of these systems remains relatively low for practical applications.
In recent years, there has been a growing interest in exploring porous organic polymer (POPs) based photocatalysts due to their inherent advantages, such as cost-effectiveness, high stability, facile separation and recovery processes.27,28 These materials have emerged as a prominent class of heterogeneous photocatalysts for selective transformations involving organic molecules in the presence of molecular oxygen.29–32 However, it remains challenging as the photocatalytic performance of most of the reported POPs is still unsatisfactory mainly due to the limited light utilization, fast recombination of charge carriers, inefficient charge generation, and charge transfer within the organic semiconductors. Addressing these limitations necessitates concerted efforts towards refining the molecular architecture of POPs to enhance photon absorption and exciton dissociation efficiencies. In this regard a novel strategy was conceived for the incorporation of donor–acceptor (D–A) units within the polymeric networks POPs.33–35
Herein, two polymeric photocatalysts with fluorene as donor unit and heptazine or triazine as the acceptor unit (named as HEP-FL and TZ-FL, respectively) were designed and fabricated using nucleophilic substitution reaction between 2,5-diamino fluorene and heptazine chloride or triazine chloride aiming at increased charge separation and high photocatalytic performance. Heptazine and triazine are highly electron-deficient units and act as excellent acceptors. They are the main repetitive units and the primary active centres within polymeric graphitic carbon nitride (g-C3N4), possess notable characteristics including high nitrogen density, which contributes to the photocatalytic activity of g-C3N4 by providing a greater number of reactive sites for chemical transformations.36 Additionally, heptazine and triazine possess π-conjugated systems leading to their interesting electronic and optical properties.37,38 By varying the acceptor unit of the polymeric photocatalysts, the electron affinities can be readily modulated, leading to tunable band structures and exciton binding energies. The correlation between molecular structures and optoelectronic properties of organic semiconductors is unveiled by a series of advanced spectroscopic and electrochemical measurements. Both of these were employed for the chemo-selective photocatalytic oxidation of sulfides to sulfoxide under blue light irradiation using molecular oxygen as an oxidant and water as solvent. The optimal sample, heptazine-containing photocatalyst HEP-FL exhibits efficient charge separation efficiency, thanks to improved electron delocalization and reduced exciton binding energy, resulting in superior photocatalytic activity of HEP-FL over TZ-FL. To the best of our knowledge, this is the first study that features the heterogeneous metal-free polymeric network for the photocatalytic selective aerobic oxidation of sulfides to sulfoxides using water as solvent. We anticipate that these findings will facilitate new possibilities for the development and implementation of environmentally conscious and sustainable protocols for selective organic transformations.
The chemical structure of these polymeric networks was initially scrutinized using solid-state 13C CP/MAS NMR, confirming the successful integration of heptazine and triazine units in the polymeric network. The peaks observed at 166 and 168 ppm correspond to the heptazine and triazine carbons of HEP-FL and TZ-FL, respectively where the chlorine atoms are substituted by fluorene moiety forming a new C–N bond (Fig. 1a).39,40 The peak of heptazine carbon bonded to three nitrogen atoms, appeared at 156 ppm. The aromatic carbons of fluorene moiety gave rise to peaks in the range of 120–150 ppm. The peak at 37 ppm indicated the methylene carbons of fluorene.
Further, the successful synthesis of HEP-FL and TZ-FL was corroborated using the FTIR technique (Fig. 1b). The unambiguous indication of the presence of the heptazine and triazine moiety in the polymeric networks was demonstrated by breathing mode vibration at 800 cm−1 and 796 cm−1, respectively. In contrast, the absence of the C–Cl stretching vibration at 942 cm−1 and 850 cm−1 in the case of HEP-FL and TZ-FL, respectively served as evidence that heptazine chloride and triazine chloride efficiently underwent substitution.40 Moreover, the peaks at 1620 cm−1 corresponded to the characteristic peak of CN in the heterocycles. This along with the aromatic vibrations of FL between 1470 to 1600 cm−1 validated the presence of both the precursors in their respective polymeric network. Additionally, the high-resolution C 1s spectrum of HEP-FL showed peaks at 284.4 eV and 288.0 eV and TZ-FL showed peaks at 284.4 eV and 287.6 eV corresponding to C–C/C
C and C
N linkages, respectively. N 1s high-resolution XPS spectrum of HEP-FL was fitted into three peaks at 398.4 eV (C
N of heptazine), 399.7 eV (C3–N), and 400.5 eV (C–N) (Fig. 1d). For TZ-FL, the N 1s XPS spectrum was deconvoluted into three peaks at 398.1 eV (C
N triazine), 399.5 eV (C–N), and 400.2 eV (N–H) (Fig. 1f). The thermal and chemical stabilities of the synthesized polymers were then characterized by thermogravimetric analysis (TGA) and FTIR measurements. The thermogravimetric analysis (TGA) carried out under the N2 atmosphere showed that HEP-FL is thermally stable up to 540 °C, whereas the TF-FL is stable up to 300 °C (Fig. S3†). To check their chemical stabilities, the as-synthesized polymeric networks were immersed under different solvents for 3 days and then recorded the FTIR spectra of the collected powder (Fig. S4 and S5†). The main peaks in FTIR spectra of all the samples soaked in THF, dioxane, hexane, acetonitrile (ACN), methanol (MeOH), ethanol (EtOH), dichloromethane (DCM), dimethyl sulfoxide (DMSO), acetone, water, 6 N HCl and 6 N NaOH respectively, appear at the same wavenumber indicating that both HEP-FL and TZ-FL possess high chemical stability in wide organic solvents (Fig. S6 and S7†). The morphologies of the synthesized polymeric network were investigated using FESEM (Fig. 1g and h). They both demonstrate aggregated particle-like morphology with irregularity in the structure and absence of long-range order. Further, the broad peak obtained in the PXRD spectra revealed that both HEP-FL and TZ-FL are amorphous in nature (Fig. S8†). The disorderly growth of the polymeric networks observed could be attributed to the irreversible kinetic control exhibited during the polymerization process.39
Next, the porous characteristics of these polymeric networks were analyzed by N2 physisorption measurements at 77 K. Both HEP-FL and TZ-FL showed characteristic type-IV isotherm indicating the mesoporous nature of the polymeric networks (Fig. S9†). The Brunauer–Emmett–Teller (BET) specific surface areas of HEP-FL and TZ-FL were found to be 72 m2 g−1 and 58 m2 g−1, respectively (Fig. S10†). The larger surface area of HEP-FL compared to TZ-FL could be attributed to the rigid structure of heptazine moiety which is composed of three fused triazine rings.40
Further, to examine their light-harvesting ability, the DR UV-vis technique was utilized. It was found that both of these polymeric networks absorb well in the visible range with an absorption maximum of 420 nm for HEP-FL and 460 nm for TZ-FL (Fig. 2a inset). Using the Tauc plot band gaps (Eg) of HEP-FL and TZ-FL were determined to be 2.47 eV and 1.72 eV, respectively (Fig. 2a). To determine the band potentials, Mott–Schottky analysis was carried out. The positive slope of the curve indicated that both the polymeric networks possess characteristics of n-type semiconductors (Fig. 2b and c). The X-intercept of the Mott–Schottky plot gives the value of flat band potential which is considered to lie 0.1 V below the conduction band (CB) minimum for an n-type semiconductor.41 Therefore, the CB potential (ECB) for HEP-FL and TZ-FL was found to be −0.79 V and −0.69 V vs. Ag/AgCl, respectively. These were converted into −0.59 V and −0.49 V vs. normal hydrogen electrode (NHE) respectively using the Nernst equation (ENHE = EAg/AgCl + 0.197, at pH = 7).42,43 Using the band energy equation, EVB = ECB + Eg, the valence band potential (EVB) was calculated to be 1.88 V and 1.20 V vs. NHE at pH = 7 (Fig. 2d). Both of these have the suitable band potential to reduce molecular oxygen to superoxide radical anion (O2/O2˙− −0.33 V vs. NHE at pH = 7).
![]() | ||
Fig. 2 (a) Tauc plot (inset DR UV-vis spectrum), Mott–Schottky plot of (b) HEP-FL and (c) TZ-FL, and (d) band energy diagram. |
Firstly, a suitable solvent was scrutinized for the photooxidation of sulfides. Evidently, it can be inferred from Table 1 that solvent had a significant effect on the photocatalytic performance of the polymeric catalysts. No reaction is observed in THF and chloroform as solvent (Table 1, entries 1–4). Acetonitrile (ACN) which is one of the most commonly used solvents for photocatalytic reactions gave 8% and 23% conversion of sulfide with TZ-FL and HEP-FL (Table 1, entries 5 and 6). On replacing ACN with MeOH, the conversion was found to be increased. This could be attributed to the stabilization of the persulfoxide intermediate in polar protic solvent (Table 1, entries 7 and 8).44 By adding water to MeOH (1:
1), the conversion was further enhanced (Table 1, entries 9 and 10). This indicates the important role of water in accelerating the sulfide oxidation reaction. So, this encouraged carrying out the reaction in water which is a stronger polar protic solvent and green universal solvent. The reaction was highly efficient and indeed 100% conversion of methyl phenyl sulfide was observed in just 1.3 h using HEP-FL with selective formation of methyl phenyl sulfoxide (Table 1, entry 12). No over-oxidized product i.e., methyl phenyl sulfone was formed. Similar results were found using TZ-FL as photocatalyst, however, in this case it took a longer time for >99% sulfide conversion i.e., 3.5 h (Table 1, entry 11). Fig. 3a and b show that the methyl phenyl sulfide is linearly oxidized to sulfoxide by using HEP-FL and TZ-FL respectively, while maintaining the >99% product selectivity. No over-oxidized product i.e., methyl phenyl sulfone was formed even after longer irradiation hours.
![]() | ||
Fig. 3 Time study of photocatalytic sulfide oxidation using photocatalyst (a) HEP-FL and (b) TZ-FL; water contact angle of (c) HEP-FL and (d) TZ-FL. |
S. No. | Catalyst | Solvent | Time | Conv.a (%) |
---|---|---|---|---|
Reaction conditions: 0.1 mmol of methyl phenyl sulfide, 10 mg photocatalyst, 3 mL solvent, O2 atmosphere, temperature 27 ± 0.5 °C, under 20 W blue LED light irradiation (λ = 450 nm).a Conv. (conversion) determined using 1H NMR; n.d. = not detected. | ||||
1 | HEP-FL | THF | 4 h | n.d. |
2 | TZ-FL | THF | 4 h | n.d. |
3 | TZ-FL | CHCl3 | 4 h | n.d. |
4 | HEP-FL | CHCl3 | 4 h | n.d. |
5 | TZ-FL | ACN | 4 h | 8% |
6 | HEP-FL | ACN | 4 h | 23% |
7 | TZ-FL | MeOH | 4 h | 17% |
8 | HEP-FL | MeOH | 4 h | 35% |
9 | TZ-FL | H2O![]() ![]() ![]() ![]() |
4 h | 34% |
10 | HEP-FL | H2O![]() ![]() ![]() ![]() |
4 h | 79% |
11 | TZ-FL | H2O | 3.5 h | >99% |
12 | HEP-FL | H2O | 1.3 h | >99% |
To get deeper insights into the structure-photocatalytic activity relationship and investigate the underlying reason for the better photocatalytic performance of HEP-FL compared to TZ-FL, various techniques were used. The interaction between the polymeric network and solvent (water) is an important parameter for determining the reaction kinetics and for this purpose, water contact angle measurements were carried out. As shown in Fig. 3c and d, the water contact angles of HEP-FL and TZ-FL were found to be 24.9° and 117°, respectively. A lower contact angle with water is an indicator of hydrophilic nature. The increased hydrophilicity of HEP-FL results in better interaction between catalyst and substrate leading to efficient charge transport.
The charge separation and transfer ability of any photocatalyst determines the fate of its photocatalytic performance. The steady-state photoluminescence (PL) spectra of HEP-FL and TZ-FL showed their emission maxima at 610 nm and 640 nm respectively (Fig. 4a). HEP-FL was found to have much lower PL intensity as compared to TZ-FL. Additionally, the lifetime of charge carriers was determined using time-resolved fluorescence lifetime decay spectroscopy (Fig. 4b). The decay spectra of HEP-FL and TZ-FL were fitted biexponentially, resulting in an average fluorescence lifetime of 3.41 ns and 2.71 ns, respectively. The two distinct time constants, namely, τ1 and τ2 represents the instantaneous relaxation (or the thermal relaxation) which corresponds to the non-radiative recombination and slow decay component which is associated with radiative recombination. Since the relaxation lifetime is inversely proportional to the recombination efficiency, so the longer relaxation time corresponds to the lesser recombination. It is evident from the TRPL data that there is minimised non-radiative and radiative recombination in HEP-FL than TZ-FL. Hence, there will be a greater number of charge carriers available in HEP-FL to carry out the photocatalytic process. This decrease in the PL intensity and longer fluorescence lifetime of HEP-FL as compared to TZ-FL implies the enhanced charge separation and lower recombination of charge carriers in HEP-FL. This could be explained based on the fact that heptazine has more electron-withdrawing ability in comparison to triazine. Therefore, heptazine being a better acceptor than triazine forms a superior donor–acceptor-based polymer with increased charge separation.
Further, to investigate the effect of acceptor units on the generation of charge carriers, charge transfer dynamics, and optoelectronic properties, electron paramagnetic resonance (EPR), transient photocurrent and (photo)electrochemical studies, respectively were employed. Upon visible light irradiation, HEP-FL displayed a more intense EPR signal in contrast to TZ-FL which demonstrates its superior ability to photogenerated electrons generation (Fig. 4c). HEP-FL exhibited a higher photocurrent response than TZ-FL under several cycles of intermittent on–off light experiments (Fig. 4d). The photocurrent response is positively related to enhanced generation and separation of photogenerated charge carriers in HEP-FL. Additionally, the reaction dynamics were analyzed using electrochemical impedance spectroscopy (EIS). As shown in the Nyquist plot, the arc radius for HEP-FL is much smaller than that of TZ-FL which indicates the lesser resistance to the charge carriers and thereby enhanced charge mobility in the case of HEP-FL (Fig. 4e).45 Moreover, we performed the LSV experiment in the presence of thioanisole to look into the charge transfer dynamics. As shown in Fig. 4f, HEP-FL shows increased anodic current as compared to TZ-FL which indicates HEP-FL facilitates better charge transfer for sulfide oxidation. All these experimental results unveil the crucial impact of monomer engineering in structuring the polymeric networks. Replacing the triazine with heptazine unit into the donor–acceptor-based polymeric network promotes electron delocalization and boosts charge separation which ultimately leads to better photocatalytic performance.
S. No. | Substrate | Product | Time (h) | %Conv.a (%sel.) |
---|---|---|---|---|
Reaction conditions: 0.1 mmol of sulfide, 10 mg photocatalyst (HEP-FL), 3 mL H2O, O2 atmosphere, temperature 27 ± 0.5 °C, under 20 W blue LED light irradiation (λ = 450 nm).a Conv. (conversion) and selectivity (sel.) determined using 1H NMR. | ||||
1 |
![]() |
![]() |
1.3 | >99 (>99) |
2 |
![]() |
![]() |
1.0 | >99 (99) |
3 |
![]() |
![]() |
1.3 | >99 (99) |
4 |
![]() |
![]() |
1.8 | >99 (>99) |
5 |
![]() |
![]() |
2.0 | 99 (99) |
6 |
![]() |
![]() |
3.0 | 98 (>99) |
7 |
![]() |
![]() |
4.0 | 94 (>99) |
8 |
![]() |
![]() |
5.0 | 89 (>99) |
9 |
![]() |
![]() |
2.5 | 99 (98) |
10 |
![]() |
![]() |
2.0 | >99 (98) |
11 |
![]() |
![]() |
1.0 | >99 (>99) |
12 |
![]() |
![]() |
0.8 | >99 (>99) |
In addition, various green metrics parameters were calculated for the model reaction which are provided in Table S2.† To our delight, promising values of the green metric parameters were obtained which proves the environment-friendliness and sustainability of this photocatalytic reaction. Moreover, the green metrics for some of the reported catalysts were calculated and compared with those of our catalyst (Table S3†). Clearly, our catalyst outperformed most of these catalysts in terms of green metrics values and reaction conditions thus representing a significant step forward in developing greener catalytic processes.
S. No. | Conditions | Conva (%) |
---|---|---|
Reaction conditions: 0.1 mmol of methyl phenyl sulfide, 10 mg photocatalyst (HEP-FL), 3 mL H2O, O2atmosphere, temperature 27 ± 0.5 °C, under 20 W blue LED light irradiation (λ = 450 nm).a Conv. (conversion) determined using 1H NMR; n.d. = not detected. | ||
1 | Dark | n.d. |
2 | Without catalyst | n.d. |
3 | Under air | 94% |
4 | KI (h+ scavanger) | 13% |
5 | p-BQ (O2˙− scavanger) | 65% |
6 | NaN3 (1O2 scavanger) | 48% |
7 | IPA (OH˙ scavanger) | >99% |
Furthermore, the generation of reactive oxygen species i.e., O2˙− and 1O2 was confirmed by in situ EPR experimental studies. DMPO was utilized to trap the superoxide radical.46 Under dark conditions, no signal was observed in the EPR spectra (Fig. 5a). On irradiation of light for 10 min, a quadruple signal was indeed observed corresponding to adduct formed between DMPO and O2˙−.46 For trapping singlet oxygen, TEMP was used. No signal was observed in the dark, but upon light irradiation, a triplet signal was observed corresponding to TEMPO which is formed by trapping of 1O2 by TEMP (Fig. 5b).46 Since the reaction was carried out using water as the solvent which itself can act as a source of oxygen and lead to simultaneous production of H2O2. To investigate this, the iodometric technique using UV-vis spectroscopy was used which confirmed the presence of H2O2 in the reaction mixture (Fig. S11, experimental details in ESI†) thereby demonstrating that water is also acting as a source of the oxygen atom for generation of sulfoxide.31 To validate this further the experiment was carried out in the absence of oxygen i.e., under Argon atmosphere where 42% conversion of methyl phenyl sulfide to corresponding sulfoxide (selectivity >99%) was observed in 1.3 h using HEP-FL as photocatalyst. This confirms that water also acts as the source of oxygen for sulfide oxidation. The protons of water were reduced to produce H2 which was detected using gas chromatography (GC) technique.
![]() | ||
Fig. 5 EPR detection of in situ generated (a) O2˙− with DMPO, (b) 1O2 with TEMP over HEP-FL, and (c) recyclability studies of HEP-FL. |
Based on the preceding investigations, the plausible mechanism for photocatalytic sulfide oxidation is delineated in Scheme 2. Upon blue light irradiation, the photocatalyst is excited to produce the photogenerated electrons and holes. The holes oxidize sulfide (I) to sulfide radical cation (II). The electrons on the other hand by single electron transfer (SET) to molecular oxygen (3O2) produce superoxide radical anion (O2˙−). The oxygen for the formation of sulfoxide can come from two sources: (i) Molecular oxygen or (ii) water. Based on these two possible pathways have been proposed (pathway 1 and pathway 2). In pathway 1 in which molecular oxygen acts as oxygen source for sulfoxide formation, the O2˙− radical reacts with (I) to produce persulfoxide anion (III) intermediate.26 Moreover, singlet oxygen (1O2) which is the ROS species generated by energy transfer, can combine with sulfide (I) to directly produce intermediate (III) which on subsequent proton abstraction gives peroxide cation intermediate (IV) (R2S+–OOH) and finally the desired sulfoxide.47 In pathway 2, the water acts as a source of oxygen for sulfoxide formation which was confirmed by the simultaneous production of H2O2 during the photocatalytic reaction (Fig. S11†).31 Herein, the sulfide radical cation (I) is hydrolyzed to form intermediate (V).31 Superoxide ion which is formed by the reduction of oxygen, on subsequent abstraction of a proton (H+) and H˙ radical from intermediate (V and VI), produces H2O2 and desired sulfoxide.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d4gc03255a |