Meng-De
Dai
,
Qian
Zhang
,
Hao
Dong
and
Ya-Wen
Zhang
*
Beijing National Laboratory for Molecular Sciences, State Key Laboratory of Rare Earth Materials Chemistry and Applications, PKU-HKU Joint Laboratory in Rare Earth Materials and Bioinorganic Chemistry, College of Chemistry and Molecular Engineering, Peking University, Beijing 100871, China. E-mail: ywzhang@pku.edu.cn; Fax: +86-10-62756787; Tel: +86-10-62756787
First published on 21st December 2023
Ternary sulfides have been widely studied for photocatalytic applications recently due to their flexible chemical composition and feasible band structure regulation. Theoretical research indicates huge potential of AgBiS2 in photocatalysis despite the lack of experimental data. Herein, single crystalline AgBiS2 hollow octahedrons were developed for CO2 photoreduction with amorphous ZIF-67 frameworks as outer layers. The predominant exposure of (111) planes and central cavities endowed AgBiS2 hollow octahedrons with sufficient light harvesting and electron transfer capability. The core–shell AgBiS2@ZIF-67 heterostructure significantly facilitated the separation of photogenerated carriers on the interface and electron accumulation around the active sites, further inducing stronger electrostatic attraction between ZIF-67 and ruthenium bipyridine complexes as photosensitizers. In consequence, AgBiS2@ZIF-67 heterostructures with medium thickness of outer layers exhibited the optimum photocatalytic efficiency towards CO2 photoreduction with the average CO and H2 production rates of 2.27 mmol gcat−1 h−1 and 0.78 mmol gcat−1 h−1, which qualified AgBiS2 hollow octahedrons as a universal platform for cocatalyst loading in heterogeneous catalysis.
It is well established that metal sulfide semiconductors with narrow band gaps normally have advantages in light harvesting and charge transfer in heterogenous catalysis. Though some catalysts are incapable of performing the photocatalytic reaction independently due to insufficient band gaps, the introduction of ruthenium and cobalt complexes can effectively compensate for the drawbacks of metal sulfides.5,6 Meanwhile, binary metal sulfides have been thoroughly studied to date and further investigation on sulfide-based photocatalysts should focus on the fabrication of ternary and quaternary sulfides, such as CuGaS2, CuIn5S8, ZnIn2S4 and Cu2ZnSnS4, which might contribute to the discovery of materials with novel morphology and distinct band structure.20–23 Recently, AgBiS2 nanocrystals have been found to possess extremely high absorption coefficient and thus applied to sensitized solar cells with positive results.24,25 As an earth-abundant and non-toxic ternary metal sulfide, AgBiS2 can absorb most of the light in the visible region and generate adequate electrons under mild conditions.26–31 It is therefore reasonable to speculate that AgBiS2 should have great potential in CO2 photoreduction.31–33
Herein, for the very first time, we present an octahedron-shaped AgBiS2 hollow nanostructure coated with a thin layer of ZIF-67 frameworks as the cocatalyst for a typical CO2 photoreduction reaction driven by [Ru(bpy)3]2+ as the photosensitizers. In this case, AgBiS2 hollow octahedrons (ABS-HO) substantially served as a neutral platform for loading Co(II) active sites and assisting the adsorption of aqueous [Ru(bpy)3]2+ ions at the same time, which promoted not only the reaction rate but also the long-term stability. Notably, hollow octahedron nanostructures included two apparent characters: existence of central cavities and major exposure of {111} facets. On the one hand, large cavities enabled multiple reflections and scattering of incident light, which was beneficial to sufficient utilization of solar energy.34–36 On the other hand, (111) polar terminations solely consisting of Ag or S atoms were expected to exhibit a metallic character and hence able to provide an ideal interface for initial accumulation and subsequent transfer process of photoinduced electrons, as revealed by first-principles studies.33 In short, ABS-HO should be competent to function as a photoactive support for potential cocatalysts. To our knowledge, ZIF-67 frameworks contained multiple coordinatively unsaturated metal sites and specialized in CO2 conversion to CO under visible light illumination, which were thus selected to load onto the surface of ABS-HO for enhanced physical and chemical adsorption of CO2 molecules.37–39 To explore the specific charge transfer behavior at the interface of core–shell AgBiS2@ZIF-67 nanocrystals, various characterization methods were applied and based on the experimental results it could be inferred that the significantly improved photocatalytic performance of AgBiS2@ZIF-67 heterostructures resulted from the extraordinary photoelectrochemical properties of ABS-HO cores as well as boosted charge separation efficiency on the interface.
For the preparation of ZIF-67, 400 mg of 2-methylimidazole was dissolved in 16 mL of methanol followed by the addition of 4 mL of methanol with 80 mg of Co(NO3)2·6H2O while the remaining steps were the same as above.
According to first-principles studies, Wulff shaped AgBiS2 inclines to expose not only (100) type nonpolar surfaces but also (111) type polar terminations, which further leads to the morphology of truncated cubes in theory.33 In terms of catalyst design, predominant exposure of polar surfaces can significantly improve the adsorption and mobilization of both photoactive and photoinactive species, including reactants, photosensitizers and cocatalysts. Since {111} crystal facets are close packed planes solely consisting of either Ag, Bi or S atoms, the hollow octahedron shaped nanostructure undoubtedly maximizes polar terminations with high surface energy, which should be conducive to potential catalytic applications.
To fulfill the most exposure of polar surfaces, KBr and PVP were both indispensable for the anisotropic growth of ABS-HO. Inspired by the controllable synthesis of silver nanocubes, Br− ions and PVP molecules were introduced in the EG-based system to regulate the growth kinetics of AgBiS2 nanocrystals.40–42 In consequence, additive agents effectively altered the growth rates of nanostructures along 〈100〉 and 〈111〉 directions through the selective interaction with different crystallographic planes. Notably, the (111) polar terminations might show active chemical properties under ambient conditions despite the fact that ABS-HO was the most stable species in the reaction medium.
In order to unravel the evolution mechanism during the solvothermal reaction, a series of AgBiS2 nanocrystals were prepared in time sequence, as shown in Fig. 2a–f. The aggregates observed in ABS-20 were at least 60 nm in size, which were composed of multiple primary nuclei. The basic polyhedron units with rough edges began to appear in ABS-40 with an approximate size of 60–70 nm. Subsequently, with progressive sharpening of edges and corners, the octahedron shaped nanostructures first came into existence in ABS-60. Within the next hour, hollow octahedrons continued to enlarge with interior cavities, whose edge lengths ranged from ca. 75 nm to 175 nm.
Fig. 2 TEM images of (a) ABS-20 (nuclei), (b) ABS-40 (particles), (c) ABS-60, (d) ABS-80, (e) ABS-100 and (f) ABS-120. (g) PXRD patterns of AgBiS2 prepared in time sequence. |
The characteristic diffraction peaks in PXRD patterns of samples are basically consistent with standard AgBiS2 patterns of the cubic phase (01-089-2045), further confirming the phase purity during the entire crystal growth process (Fig. 2g). However, it is worth noting that a slight shift of diffraction peaks toward lower angles can be found in the patterns of ABS-20 and ABS-40, which presumably originate from small-sized nanocrystals with partial lattice expansion. The relative intensities of the diffraction peak at 27.5° in correspondence with {111} facets also appear to be much lower for ABS-20 and ABS-40 than other samples. This phenomenon demonstrates that primary nuclei with poorer crystallinity and enlarged d-spacing suffer from serious atomic disorder on the {111} facets, probably due to non-metal doping.43 By contrast, the diffraction peaks of other samples simply coincide with the standard pattern. Since close packed (111) planes are highly ordered atomic layers, predominant exposure of (100) planes at the early stage of crystal growth should be a kinetically driven result. It can be inferred that Br doping mainly occurs at the nucleation and aggregation stage followed by slow anion substitution during the remaining reaction time.
To confirm this view, high resolution XPS spectra of ABS-20, ABS-60, ABS-120 and ABS-HO were measured to determine the oxidation states of constituent elements. The XPS spectra of Ag 3d, Bi 4f, S 2p and Br 3d regions are demonstrated in Fig. 3a–c. In the Bi 4f spectra overlapping with the S 2p region, two strong peaks appear at 162.6 eV and 157.3 eV for ABS-120 and ABS-HO. The corresponding peaks emerge at 162.7 eV and 157.4 eV for ABS-60. In addition to two major peaks at 163.3 eV and 158.0 eV, a pair of satellite peaks can be observed at 164.3 eV and 159.0 eV for ABS-20, which derives from the antisite defects of Bi atoms in the primary nuclei.26,27 As presented in the same spectra, two weak peaks at 161.4 eV and 160.3 eV belong to S 2p1/2 and S 2p3/2 of S2− for ABS-120 and ABS-HO, which shift to 161.5 eV and 160.4 eV for ABS-60. The corresponding peaks further shift to 161.9 eV and 160.8 eV for ABS-20. The Ag 3d spectra show doublet peaks at 372.8 eV and 366.8 eV for ABS-120 and ABS-HO, which should be assigned to Ag 3d3/2 and Ag 3d5/2 of Ag+.26,27 The peaks observed in the Ag 3d spectra of ABS-60 are located at 372.9 eV and 366.9 eV, further shifting to 373.5 eV and 367.5 eV for ABS-20. In general, the oxidation states of Ag, Bi and S can be regarded as +1, +3 and −2 based on the above results except for ABS-20. It is also worth mentioning that ABS-60 shows slightly higher binding energies than ABS-120 and ABS-HO. As for the Br 3d spectra, the relative intensities of peaks monotonically decrease with the extension of reaction time and eventually vanish in the spectra of ABS-HO. Hence, a certain conclusion can be drawn that Br doping can make a significant impact on the formation of AgBiS2 nuclei, directly inducing atomic defects and lower electron density around Ag, Bi and S atoms. This phenomenon can be attributed to the particular competition between slow release S2− ions from thiourea and excess Br− ions in the solution. Considering the much lower solubility of AgBiS2, S substitution should be favorable in thermodynamics.
Despite the above constituent elements, characteristic peaks of C, N and O can be also detected in the XPS spectra (Fig. S1 in the ESI†), indicating strong adsorption of PVP molecules on the surface of AgBiS2 nanocrystals. In addition, FTIR spectra can confirm the existence of PVP molecules as well (Fig. S2 in ESI†). The broad absorption band ranging from 3600 cm−1 to 3000 cm−1 evidently belongs to the stretching vibration of O–H bonds from water molecules adsorbed on the surface. The absorption peaks located at 2916 cm−1, 1652 cm−1, 1437 cm−1 and 1274 cm−1 can be attributed to the vibration of C–H bonds, CO bonds, methylene groups (–CH2–) and peptide bonds (–CO–NH–).42 On account of XPS and FTIR spectra, PVP molecules attached to the (111) planes of AgBiS2 nanocrystals should be considered irremovable during the solvothermal reaction while doped Br− ions can easily dissolve back into the solution through anion exchange.
The optical properties of AgBiS2 nanocrystals with different sizes were thoroughly investigated via UV-vis-NIR diffuse reflectance spectroscopy (Fig. 3d). Basically, AgBiS2 nanocrystals can absorb most of light in the ultraviolet and visible region. However, the absorption edges gradually shift toward the near infrared region as the reaction time prolongs. This monotonic trend is in accordance with TEM images and PXRD patterns of corresponding samples. In other words, the uncommon behavior of ABS-20 and ABS-40 simply arises from the small-sized character of nanocrystals, which causes not only poorer crystallinity but also enlarged band gaps thanks to the quantum confinement effect. By comparison, AgBiS2 nanocrystals obtained from 60 min to 120 min have homologous structural and optical properties. Notably, every single spectrum can be transformed to the corresponding Tauc plot by using a conversion formula: (αhν)1/r = C(hν − Eg), where α, h, ν and C represent the absorption coefficient, Planck constant, frequency of incident light and proportional constant. The r value should be 1/2 for direct semiconductors or 2 for indirect semiconductors. The consequent band gap values can be then approximated by extrapolating the linear region to the abscissa. Regarding AgBiS2 as an indirect band gap semiconductor,32 the corresponding band gaps of ABS-20, ABS-40, ABS-60, ABS-80, ABS-100 and ABS-120 ought to be 1.20 eV, 0.90 eV, 0.77 eV, 0.76 eV, 0.75 eV and 0.75 eV (Fig. S3 in ESI†). It is clear that the quantum confinement effect primarily influences ABS-20 and ABS-40 as kinetically driven products.
To unravel the mechanism of crystal growth, several control experiments were conducted for the crystal growth process without various additive agents. TEM images display that AgBiS2 nanorods were generated for both circumstances in the absence of KBr or PVP (Fig. S4 in ESI†). Hence, it is reasonable to presume that Br− ions and PVP molecules can stabilize (111) planes after initial nuclei self-assemble into basic polyhedrons. In detail, doped Br− ions should be distinguished from adsorbed Br− ions regarding their functions in facet control. During the nucleation and aggregation process, Br− ions doped in the lattices of AgBiS2 nanocrystals evidently tend to suppress the selective growth of close packed (111) planes according to PXRD patterns. By contrast, Br− ions adsorbed on the surface can lower the energy of (111) planes with Ag or Bi terminations by electrostatic attraction.
On the one hand, small-sized adsorbates are easier to remove by deionized water and ethanol than long-chain macromolecules, which explains the fact that C, N and O show characteristic peaks in the XPS spectra of ABS-HO while signal of Br cannot be detected. On the other hand, it is more accessible for Br− ions to interact with small-sized nuclei than PVP molecules at the beginning of crystal growth.26,27,41 The nucleation process involves the participation of Br− ions, which limits the concentration of free Ag+ ions in the solution and therefore inhibits the overall reaction.41 Meanwhile, deficient S2− ions endow Br− ions with chances of doping in the lattice as counter ions. It is worth noting that doped Br− ions can easily detach from the lattice without affecting the phase purity of cubic AgBiS2.
Based on the structural and elemental analyses of samples, a plausible evolution mechanism can be proposed, as presented in Fig. 4. First, rapid nucleation induces partial Br doping in the cubic AgBiS2 lattices and further influences the diffraction peaks in the PXRD pattern. Owing to the strong passivation of Br− ions, subsequent growth basically depends on anion exchange in the solution, which conduces to the formation of small aggregates at this stage. The aggregates incline to assemble into basic polyhedron units by oriented attachment rather than grow directly through Ostwald ripening.44 As edges and corners of polyhedron units are sharpened progressively, neighbouring pores will naturally converge into a central cavity. Since enlarged cavities lead to more exposure of (111) planes, continuous growth of hollow octahedrons should be a thermodynamically favorable result. This process perhaps involves anion transfer from the inner side to the outer surface through the lattices followed by deposition with cations.
Fig. 5 (a) TEM image, (b) HRTEM image and (c)–(i) HAADF-STEM with EDX elemental mapping images of AZ-20. |
In addition, TEM images of AZ-10, AZ-40 and ZIF-67 were also captured for comparison (Fig. S6 in ESI†). The outer shell of AZ-20 appears to be thicker than AZ-10 and thinner than AZ-40 while ZIF-67 shows the typical morphology of rhombic dodecahedra. According to the PXRD patterns, the characteristic diffraction peaks of as-prepared ZIF-67 are consistent with the simulated pattern. The relative intensities of diffraction peaks within the small angle region increase slightly from AZ-10 to AZ-40, suggesting poor crystallinity of ZIF-67 on the shell (Fig. S7 in ESI†).45 FTIR spectra confirm the existence of 2-methyimidazole in AZ-20 and ZIF-67 with no obvious signal of PVP (Fig. S8 in ESI†).38,45 Furthermore, ICP-OES was performed to determine the actual contents of Co in different samples. In consequence, the approximate values of Ag:Bi:Co molar ratios in AZ-10, AZ-20 and AZ-40 were 1:1:0.2, 1:1:0.4 and 1:1:0.9, respectively.
UV-vis-NIR diffuse reflectance spectra clarify that the optical properties of ABS-HO and ZIF-67 substantially remain unchanged in the core–shell heterostructures (Fig. S9 in ESI†). The absorption peaks of ABS-HO and ZIF-67 are located at 1125 nm and 586 nm respectively, corresponding to band gaps of 0.75 eV and 1.98 eV, as revealed by Tauc plots (Fig. S10 in ESI†). Mott–Schottky tests were conducted to uncover more details about band structures of ABS-HO, AZ-20 and ZIF-67 (Fig. 6a). The curve slope of ABS-HO appears to be positive with classical n-type semiconductor characteristics while ZIF-67 shows negative curve slope with typical p-type semiconductor characteristics. The Mott–Schottky plot of AZ-20 possesses both characteristics of ABS-HO and ZIF-67, verifying the composition of two semiconductors in the core–shell heterostructures. The flat band potential can be acquired by extrapolating the linear region to the abscissa. The position of valence band maximum (VBM) can be estimated to the flat band potential for ZIF-67 as a p-type semiconductor. Likewise, the position of the conduction band minimum (CBM) can be obtained by the estimation based on the Mott–Schottky plot for n-type semiconductors.
Fig. 6 (a) Mott–Schottky plots and (b) schematic diagram for the band alignment of ABS-HO, AZ-20 and ZIF-67. |
The relative positions of VBM and CBM in ABS-HO, AZ-20 and ZIF-67 are summarized in Fig. 6b according to Tauc plots and Mott–Schottky plots. Undoubtedly, AZ-20 should be categorized as a type-II heterostructure and thus favorable for photogenerated electrons to transfer from the ABS-HO core to the ZIF-67 shell.1–4 High resolution XPS spectra were also measured to determine the direction of electron migration between ABS-HO and ZIF-67 (Fig. S11 in ESI†). In the Ag 3d and Bi 4f spectra, peaks shift to higher binding energy with the increasing content of Co, reflecting an inevitable loss of electron density. By comparison, the binding energy of Co almost remains unchanged for all the samples, revealing the steady oxidation state of +2 for Co. The binding energy of N slightly decreases from AZ-10 to ZIF-67. On account of the Fermi levels, electrons should migrate from ABS-HO to ZIF-67 spontaneously. In practice, two components seem to both suffer from electron deficiency when mixed together. This phenomenon could be ascribed to the desorption of PVP and partial oxidation of 2-methylimidazole.
During the photocatalytic tests, CO was the only carbonaceous reduction product with H2 as the by-product derived from the decomposition of water under light irradiation. The experimental results are in accordance with previous reports regarding CO2 conversion to CO initiated by Ru(II)–Co(II) complexes.10,12,36 Ru(bpy)3Cl2 can hardly trigger CO2 photoreduction reaction in the absence of cocatalysts despite its high photoexcitation efficiency. By contrast, Co(II) complexes are practically incapable of utilizing solar energy in exchange for excited electrons. In other words, the catalytic performance of Ru(II)–Co(II) complexes mostly depends on the transfer rate of electrons from Ru(II) sites to Co(II) sites.
In consequence, all of the cocatalysts can convert CO2 into CO molecules with the side reaction of hydrogen evolution except for ABS-HO showing the worst catalytic performance, which implies that Co(II) complexes should be responsible for the adsorption and activation of substrate molecules (Fig. 7a and b). However, pure ZIF-67 with theoretically more active sites shows a lower production rate than AZ-10, AZ-20 and AZ-40. In detail, AZ-20 as the best catalyst produced 54.4 μmol CO and 17.8 μmol H2 in total, which were collected during the photocatalytic test with reaction time extended to 12 h for the demonstration of superior stability. It is worth mentioning that AZ-20 and ABS-HO can work in the reaction medium continuously with basic nanostructures unchanged, as presented in TEM images (Fig. S12 in ESI†). PXRD patterns were recorded to determine the phase purity of AZ-20 after the photocatalytic test as well (Fig. S13 in ESI†). It is well established that Ru(bpy)3Cl2 would inevitably suffer from photobleaching under visible light irradiation. Hence, Ru(II)–Co(II) complexes normally function in a short test before stepwise deactivation causes serious efficiency decay.36,38 Since the rate of CO production remained steady for 12 hours, Ru(bpy)3Cl2 ought to be more stable when coupled with AZ-20 in the solution. Suppressed decomposition of Ru(bpy)3Cl2 could originate from strong attachment to the supports, which stabilizes the chromospheres on the photosensitizers.12
Fig. 7 Time-dependent (a) CO and (b) H2 productions of ABS-HO, AZ-10, AZ-20, AZ-40 and ZIF-67. (c) EIS Nyquist plots and (d) transient photocurrent spectra of ABS-HO, AZ-20 and ZIF-67. |
EIS Nyquist plots and periodic photocurrent responses were recorded to explore the carrier migration kinetics of cocatalysts (Fig. 7c and d). Among these samples, AZ-20 shows the smallest arc radius of the Nyquist plot, which represents lower charge transfer impedance and more advantageous charge transfer kinetics. By comparison, pure ZIF-67 nanocrystals with much higher impedance should have great difficulty in carrier migration. Likewise, AZ-20 also exhibits the highest photocurrent density whilst the periodic photocurrent responses of ZIF-67 can be hardly detected under the same test conditions. Therefore, ZIF-67 can barely make any contribution to either light harvesting or charge transfer under light illumination while ABS-HO as the inner core can generate and transport numerous electrons to the surface of ZIF-67 as the outer shell, further inducing strong photocurrent in AZ-20.
The average production rates of all the samples are presented in Fig. 8a for further comparison. To further investigate the origin of optimum photocatalytic performance for AZ-20, steady-state PL spectra were recorded to simulate the process of electron migration under light illumination (Fig. 8b). Upon the irradiation of monochronic incident light (450 nm), certain cocatalysts dispersed in the MeCN/TEOA/H2O solution with Ru(bpy)3Cl2 will emit strong fluorescence detected by the instrument. Interestingly, sole Ru(bpy)3Cl2 without the assistance of cocatalysts shows the lowest fluorescence intensity. The fluorescence emission of [Ru(bpy)3]2+ ions reaches the climax when coupled with ABS-HO. Furthermore, AZ-10, AZ-20 and AZ-40 can also enhance the characteristic fluorescence from [Ru(bpy)3]2+ in the solution. The relative intensity of fluorescence emission for AZ-20 appears to be lower than AZ-10 and AZ-40, which can accord with the photocatalytic performance as decay of fluorescence intensity should be mainly ascribed to electron transfer from [Ru(bpy)3]2+* to Co(II) sites. Hence, an outer shell with medium thickness can endow the catalyst with both abundant active sites on the surface and photoexcited electrons from the inner core.
Fig. 8 (a) The average CO and H2 production rates and (b) steady state PL spectra of ABS-HO, AZ-10, AZ-20, AZ-40 and ZIF-67. |
In terms of mass transfer, it should be unfeasible for TEOA and [Ru(bpy)3]2+ to reach the ABS-HO core through small pores of ZIF-67 frameworks in the heterostructures.17 Naturally, Co(II) sites on the surface ought to be responsible for the adsorption and activation of substrates or photosensitizers. The electron migration process can only occur on the interface between cores and shells or on the surface of ZIF-67 with adsorbed photosensitizers while direct charge transfer between ABS-HO and [Ru(bpy)3]2+ should be inaccessible. It is worth mentioning that even AZ-40 with the thickest outer layers shows stronger fluorescence than sole [Ru(bpy)3]2+, confirming that the ABS-HO core mainly affects [Ru(bpy)3]2+ by electron transfer rather than electric field or energy transfer. In other words, photoelectrons generated by ABS-HO would accumulate on the surface of ZIF-67 and provide a negative environment for the adsorption of [Ru(bpy)3]2+ ions by electrostatic attraction. Considering that the fluorescence intensity of [Ru(bpy)3]2+ barely changes upon the addition of ZIF-67, direct electron transfer from aqueous [Ru(bpy)3]2+ ions to the surface of p-type ZIF-67 should be unfavorable. By contrast, the negative surfaces created by ABS-HO at the photoexcited state can easily facilitate the adsorption of free [Ru(bpy)3]2+ ions in the solution and thus inhibit the quenching process induced by collision, further leading to enhanced fluorescence of [Ru(bpy)3]2+. Based on the band alignment and charge transfer kinetics, a plausible mechanism for electron transfer process is illustrated in Fig. 9a and b.
It should be mentioned that none of the samples can trigger the reaction without photosensitizers and negligible reduction products were collected during the tests. Meanwhile, all of the photocatalysts are inactive in the absence of CO2, TEOA and light irradiation, which means no detection of products under a nitrogen-protected atmosphere, sacrificial agent-free system or/and dark conditions (Fig. S14 in ESI†). Ru(bpy)3Cl2 as the sole photocatalyst exhibits relatively low CO production rate with high selectivity towards H2 evolution instead. 1H NMR spectra also clarify that none of the liquid reduction products were obtained during the aforementioned photocatalytic tests (Fig. S15 in ESI†). Basically, the pale-orange upper solution after the reaction was acetonitrile solution containing Ru(bpy)3Cl2, TEOA and H2O whilst the scarlet lower solution was Ru(bpy)3Cl2 aqueous solution mixed with TEOA and MeCN.
To sum up, ABS-HO should have remarkable potential in the regulation and optimization of active sites for different catalyst units. In this work, suitable band alignment leads to the construction of core–shell heterostructures based on cubic ABS-HO nanocrystals and amorphous ZIF-67 frameworks with enhanced photocatalytic performance, thanks to boosted carrier transfer through the type-II heterostructure. During the photocatalytic reaction, ABS-HO effectively promotes not only the reduction ability of potential cocatalysts but also the stability of expensive photosensitizers.
Footnote |
† Electronic supplementary information (ESI) available: More data on TEM images, PXRD and XPS analyses, and photocatalytic measurements of heterostructures. See DOI: https://doi.org/10.1039/d3ma00662j |
This journal is © The Royal Society of Chemistry 2024 |