Hongyu Heab,
Lulu Lia,
Ruhan Yac,
Hong Liud,
Bin Luod,
Zhipeng Li*b and
Wenhuai Tian*b
aSchool of Materials Science and Engineering, University of Science and Technology Beijing, Beijing 100083, China. E-mail: hehongyu666@126.com; 15733153822@163.com
bSchool of Materials Science and Engineering, Shunde Innovation School, University of Science and Technology Beijing, Foshan 528300, China. E-mail: zplmse@ustb.edu.cn; wenhuaitian@ustb.edu.cn
cInner Mongolia Academy of Science and Technology, Huhhot 010020, China. E-mail: YARUHANJIAN@163.com
dGuangdong Homeen Organic Silicon Material Co., Ltd, Zhaoqing 526072, China. E-mail: roben@hm-sil.com; liuhong@homeen.cn
First published on 30th July 2024
The molecular motion trajectories of silicone rubber foam (SRF) at various vinyl silicone oil viscosities were studied via molecular dynamics (MD) simulation from the perspective of all atomic molecules. The influence of different viscosities of vinyl silicone oil on interaction, compatibility, and aggregation degree of molecules was determined based on the mean square displacement, diffusion coefficient, binding energy, solubility parameter, radial distribution function, and radius of gyration. The mechanical properties of the SRF were also experimentally verified. Results revealed that as the viscosity of vinyl silicone oil increased, the mean square displacement, fractional free volume, diffusion coefficient, and solubility parameter of the system decreased, whereas its larger radius of gyration increased. Moreover, the radial distribution function showed a weaker relative interaction between molecular chains. The calculated binding energy demonstrated that the system had better compatibility at a viscosity of 0.45 Pa s. This study provided a deeper insight into the relation between the viscosity of vinyl silicone oil and mechanical properties of the SRF. As the viscosity of vinyl silicone oil increased, the changing trend in MD simulation results of elastic modulus, shear modulus, bulk modulus, and Poisson's ratio was consistent with the experimental results. The MD simulations can promote theoretical predictions and scientific basis for the design of the SRF with desired performances.
Molecular dynamics (MD) is a method to simulate the properties of materials at the micromolecular and atomic levels. It is used to study the effects and mechanisms of polymer modification because a large number of atoms or molecules are simulated on a large time scale.8–10 MD simulation explores the interactions between microscopic molecules based on the principle of statistical analysis of the arrangement and motion of atoms or molecules, which cannot be experimentally derived. Various polymer properties have been investigated via MD simulation.11,12 Pahari et al.11 found that MD simulation can be used to effectively predict the viscoelastic and thermodynamic properties of rubber. Lee et al.12 utilized MD simulation to analyze the fibrillization process and thermal stability of silicone foams by adding fibrillated microcrystalline cellulose, and the simulation result of fibrillization details was consistent with the experimental result. Wei et al.13 applied MD simulation method to investigate the mechanical properties of poly(vinyl alcohol) (PVA)/poly(acrylic acid) (PAA) blend systems. Results showed that the PVA chain formed a stronger intermolecular interaction than the PAA chain at the same quality. Zhu et al.14 studied the dynamic mechanical property of silicone rubbers with different phenyl units and phenyl contents via combining experiments and MD simulation.
Currently, the regulation of cellular structure, rheology, viscoelasticity, and aging of the SRF have been studied.15–19 Few researchers have conducted in-depth the impact of vinyl silicone oil viscosity on the performance of the SRF via all-atom molecular dynamic simulation.20,21 This article has investigated in detail the molecular motion trajectories, molecular interactions, and the crosslinking process of the SRF prepared from vinyl silicone oil with different viscosities through MD simulation. The intermolecular motion (such as mean square displacement, diffusion coefficient, fractional free volume, and cohesive energy density) and the molecular stereo configuration (radial distribution function and radius of gyration) were also investigated. The simulation results of mechanical properties and the experimental results were in contrast with each other. This research will provide theoretical basis and data support for the actual industrial production of the SRF.
Vinyl silicone oils with a viscosity of 0.45 and 200 Pa s were adopted in system I and II, respectively. Tables 1 and 2 show the experimental formulation of the SRF for systems I and II, respectively.
Component | Materials | Viscosity/Pa s | Vinyl content/% | Mole content/mol |
---|---|---|---|---|
A | Vinyl-terminated MQ silicone resin | 100 | 1.3 | 0.00241 |
Vinyl-terminated silicone oil | 10 | 0.14 | 0.000691 | |
Vinyl-terminated silicone oil | 0.45 | 0.4 | 0.00263 | |
Hydroxyl-terminated silicone oil | 0.02 | — | 0.00471 | |
B | Vinyl-terminated MQ silicone resin | 100 | 1.3 | 0.00241 |
Vinyl-terminated silicone oil | 10 | 0.14 | 0.000691 | |
Vinyl-terminated silicone oil | 0.45 | 0.4 | 0.00237 | |
Hydrogen-containing silicone oil | 0.02 | — | 0.064 |
Component | Materials | Viscosity/Pa s | Vinyl content/% | Mole content/mol |
---|---|---|---|---|
A | Vinyl-terminated MQ silicone resin | 100 | 1.3 | 0.00241 |
Vinyl-terminated silicone oil | 10 | 0.14 | 0.000691 | |
Vinyl-terminated silicone oil | 200 | 0.02 | 0.00132 | |
Hydroxyl-terminated silicone oil | 0.02 | — | 0.00471 | |
B | Vinyl-terminated MQ silicone resin | 100 | 1.3 | 0.00241 |
Vinyl-terminated silicone oil | 10 | 0.14 | 0.000691 | |
Vinyl-terminated silicone oil | 200 | 0.02 | 0.00119 | |
Hydrogen containing silicone oil | 0.02 | — | 0.064 |
The amorphous cell module was used to build the simulation box with molecules a, b, c, d, e, and f. Considering the limitation of the computer resources, the atomic number in a single molecular chain of systems was taken to be about 600–700. At the same time, the number of repeating units could not exceed 500. Therefore, it is crucial to choose the appropriate chain length of silicone rubber foam. According to Hildebrand's theory,22 the solubility parameter of silicone rubber will tend to a constant value when the degree of polymerization of silicone rubber chains exceeded a certain critical value. Reducing the scale of the repeating units by 10 times met the above conditions. Therefore, the molecular chain of molecules b, c, and f was reduced in the same proportion during the simulation process, with a reduction ratio of 10. The repeat unit of molecules b, c, and f was 52, 18, and 364, respectively. The total number of atoms in the systems I and II was 4388 and 5136, respectively. The initial density was set to 1 g cm−3. The reactive atoms on different chains were named R1 or R2 (as shown in the blue circle of Fig. 1). The cross-linked model was obtained by simulating the crosslinking process of groups R1 and R2, which were selected as the alternative crosslinks.
The force field parameters just like DREIDING and optimized potentials for liquid simulations (OPLS) will present some error at the simulation process except the temperature at 0 K.23,24 The COMPASS force field is a high-performance and powerful force field, which can predict the microstructure, molecular conformation, and thermophysical properties of polymers within a wide range of temperature and pressure. The Forcite module was applied to optimize the molecular structure with COMPASS II as the force field.25,26 During the geometric optimization process, the convergence thresholds for maximum energy change, maximum force, and maximum displacement were 0.001 kcal mol−1, 0.5 kcal mol−1 Å−1, and 0.015 Å, respectively. Then, 100 ps dynamic simulation was performed under the NPT ensemble (constant number of particles, pressure, and temperature) at 0.0001 GPa and 298 K to determine the density fluctuations until the density–time curve was stable. To release the internal stress of the system, the model was annealed at 300–500 K, with a total of 200000 steps. For further optimizing the structure, a 100 ps dynamic simulation was conducted under the NPT and NVT ensembles (constant number of particles, volume, and temperature), respectively. The precise Nose–Hoover temperature control mode and Berendsen pressure control mode were utilized in the dynamic process. The simulations were conducted at 298 K and a step size of 0.2 fs.
The energy curve of the optimized model is shown in Fig. 2. During the MD simulation of the SRF, the state of the entire simulation process must be meaningful and stable. The energy curves of these systems fluctuated in the range of ∼1–5%, indicating the effectiveness of the simulation model. These results also confirmed that the two systems reached an equilibrium state.
Fig. 2 Energy curve of the SRF versus simulation time. (a and b) NPT and NVT of system I; (c and d) NPT and NVT of system II. |
Fig. 3 Model diagram of the SRF before and after crosslinking. (a and b) Before and after crosslinking of system I; (c and d) before and after crosslinking of system II. |
According to the research of Messinger,27 it was found that the cellular microstructure had no effect on the mechanical properties of the organosiloxane foams. The mechanical properties were related to differences in molecular composition, structure, and polymer chain dynamics. This suggests that bubbles can be disregarded in simulations and that their presence does not invalidate the results. Therefore, it is reasonable to use molecular dynamic simulation without simulate bubbles in the simulation process for studying the SRF.
Components A and B were stirred in a vacuum defoaming mixer (vacuum degree of −100 kPa) at 800 rpm. The flow chart for the SRF preparation is shown in Fig. 4. The two components were completely mixed in a 1:1 mass ratio and stirred for 2 min and quickly poured into a mold at room temperature. Then, the molding plate was cured at 60 °C and post-cured at 150 °C for 15 min, yielding the SRF. Post-curing improved the degree of curing and the components reacted completely at 150 °C, which improved the mechanical properties of the SRF and eliminated any volatile substances.
There has two main methods for analyzing the mechanical properties of system, static and dynamic method in MD simulation, respectively. In the static method, the bond angle was fixed, whereas the influence of configuration entropy on the elastic constant was disregard. Contrarily, the dynamic method is time-consuming and suffers from uncertainties in the results due to strain fluctuations. Therefore, the static method was used for simulation herein.
The static mechanical properties of the SRF were measured using an electronic universal testing machine (E43.104, MTS) and an axial extensometer (ZEM5.204, ZHIXIN). A schematic of the dumbbell sample is shown in Fig. 5. The effective part of the sample was 33 mm × 6 mm × 5 mm (length × width × thickness). During the experiment, the sample was uniformly stretched with a stretching rate of 50 mm min−1. For each set of data on the materials' properties, at least five samples were tested for each system and the values were averaged.
The VTMR12-010V-I nuclear magnetic resonance (NMR) crosslinking densimeter was used to test the crosslinking density of the foaming materials. The effective detection range of the sample was φ8.5 × H20 mm. The magnetic field intensity was set to 0.5 ± 0.05 T. The crosslinking density was determined at 30 °C. LX-C shore hardness testers were utilized to measure the shore hardness (shore C) of the SRF. The tensile strength and elongation at break of the SRF were tested using the WDW-10 universal testing machine at a tensile rate of 500 mm min−1. The sample was stretched uniformly during the experiment. Five samples were measured, and the average value was used as the final value in the experiment.
MSD = 〈|ri(t) − ri(0)|2〉 | (1) |
Fig. 6 shows the MSD curves of molecular chains of different components in the two systems at 298 K. A linear correlation existed between the MSD and the simulation time, indicating that the diffusion system was in a state of normal diffusion. MSD curve showed an upward trend as the simulation time increased. Fig. 6(a) and (b) show that the MSD of system II is smaller than that of system I. To accurately analyze the MSD curves, the MSDs of functional groups in the system were determined (Table 3). The MSD of the Si–H bond was the highest, whereas those of –CHCH2 in molecules c and f is relatively smaller, primarily because hydrogen-containing silicone oil has shorter molecular chains. Thus, the molecules can easily move, which results in a larger MSD. Contrarily, vinyl silicone oil has longer molecular chains, which cannot move easily, resulting in a smaller MSD. Moreover, system I has a shorter molecular chain and a larger free volume than system II, which facilitates easier molecular chain movement. A shorter molecular chain length implies that the resistance of motion in the system is lower, and the MSD of the molecular chain is the larger.
Component | MSD/Å2 | |
---|---|---|
System I | System II | |
Si–O–Si (silicon resin) | 31.99 | 21.62 |
–CHCH2 (vinyl silicone oil of 0.45 Pa s) | 16.6 | — |
–CHCH2 (vinyl silicone oil of 10 Pa s) | 28.59 | 20.26 |
–CHCH2 (vinyl silicone oil of 200 Pa s) | — | 18.30 |
Si–H (hydrogen containing silicone oil) | 37.39 | 24.43 |
Si–OH (hydroxy silicone oil) | 18.37 | 17.45 |
(2) |
Table 4 shows the D of the SRF in systems I and II. It can be seen that system I had a larger D. This is due to the 0.45 Pa s vinyl silicone oil has short molecular chains, relatively small molecular weight, and large free volume within the system, allowing easy molecular chains movement.
Component | D/(Å2 ps−1) | |
---|---|---|
System I | System II | |
Si–O–Si (molecule a) | 0.0352 | 0.0189 |
–CHCH2 (molecule b) | 0.0314 | 0.0184 |
–CHCH2 (molecule c) | 0.0173 | — |
Si–OH (molecule d) | 0.0182 | 0.0168 |
Si–H (molecule e) | 0.0477 | 0.0215 |
–CHCH2 (molecule f) | — | 0.0196 |
(3) |
Fig. 7 shows the free volume morphology of the SRF with different vinyl silicone oil viscosities. The free and occupied volume of the SRF are denoted in blue and gray, respectively. The FFV of the SRF with different viscosities of vinyl silicone oil is shown in Table 5. Fig. 7 and Table 5 show that the free volume and FFV decrease as of vinyl silicone oil viscosity increases. This is due to the 200 Pa s vinyl silicone oil has a long molecular chain, relatively large molecular weight, larger volume of polymer chains, and smaller FFV. A larger FFV allows for more active movement of molecules within a larger space, thereby increasing the diffusion coefficient.36 This finding is consistent with the previous results of MSD and D values.
Fig. 7 Free volume morphology of the SRF with different vinyl silicone oil viscosities. The blue denotes the area of free volume. (a) System I; (b) System II. |
Systems | System I | System II |
---|---|---|
Free volume/A3 | 11252.53 | 13069.62 |
Occupied volume/A3 | 41551.33 | 48563.77 |
FFV/% | 21.31 | 21.21 |
Ebinding = −Einter = −(Etotal − E–CHCH2 − ESi–OH − ESi–H) | (4) |
Tables 6 and 7 show the free energies of different components and the Ebinding of systems I and II. After simulation, the Ebinding of the SRF prepared using vinyl silicone oils of 0.45 and 200 Pa s were 551.52 and −604.30 kcal mol−1, respectively. The absolute value of the Ebinding in system II was slightly higher than that in system I, with a difference of ∼52.78 kcal mol−1. Based on the sign of the Ebinding, the compatibility of two components of the SRF can be confirmed.39 A negative Ebinding indicates that the components have a poor compatibility, and a positive Ebinding indicates their good compatibility. A larger positive Ebinding implies the components of the two systems will have better compatibility.40 The stability of the SRF is affected by the magnitude of Ebinding. A larger absolute value of the Ebinding will enhance the system stability.41 Moreover, the Ebinding is influenced by the molecular chain length. System I has better compatibility for the two components due to the positive Ebinding and shorter molecular chains; therefore, the molecules are compatible with each other in this system.
Functional group/item | Free energy/(kcal mol−1) | |
---|---|---|
System I | System II | |
Etotal | −34545.413 | −36946.094 |
Si–O–Si (Ea) | −11581.263 | −4884.269 |
–CHCH2 (10 Pa s) (Eb) | −8343.170 | −3381.280 |
–CHCH2 (0.45 Pa s) (Ec) | −7727.943 | — |
–CHCH2 (200 Pa s) (Ef) | — | −986.613 |
Si–OH (Ed) | −2344.130 | −1693.140 |
Si–H (Ee) | −3997.385 | −26605.088 |
Item | Ebinding/kcal mol−1 |
---|---|
System I | 551.52 |
System II | −604.30 |
(5) |
The solubility parameter (δ) is applied to determine the compatibility and dissolution characteristics of different components or polymers. It is the square root of the CED and can be determined for the SRF as follows:40
(6) |
Table 8 shows that the CED and δ of the SRF prepared using vinyl silicone oils of 0.45 and 200 Pa s are 1.717 × 108 J m−3 and 13.104 (J cm−3)1/2 as well as 1.540 × 108 J m−3 and 12.408 (J cm−3)1/2, respectively. As the viscosity of the vinyl silicone oil increases, the CED and δ of the SRF decrease, indicating weak interaction between the SRF components. The higher the CED and δ, the better the compatibility between the components in the SRF. Thus, system I has better compatibility than system II. This finding is consistent with the Ebinding results.
Item | CED/(J m−3) | δ/(J cm−3)1/2 |
---|---|---|
System I | 1.717 × 108 | 13.104 |
System II | 1.540 × 108 | 12.408 |
Moreover, δ decreases with increasing viscosity of vinyl silicone oil and the number of repeating units. This result is consistent with that reported previously,40 where the δ of NR and SBR gradually decreased as the number of Nunit (chain repeating units) increased.
(7) |
Fig. 8 shows the RDFs of the SRF for the vinyl silicone oil viscosities of 0.45 and 200 Pa s, respectively. The RDFs of other atoms (such as Si–OH and –CHCH2) found around the Si–H in hydrogen-containing silicone oil as the central atom has a significant peak at a certain distance. This indicates that Si–H has a strong attraction to other atoms around this distance. Moreover, the RDFs of the five components in the SRF are similar in the number, distribution, and patterns of peaks, but the peak values are different.
Fig. 8 Total g(r) of Si–H for different viscosities of vinyl silicone oils; the plots on the left and right represent different distances (r). (a) System I; (b) System II. |
As vinyl silicone oil viscosity increases, the SRF forms looser aggregates and a relatively large g(r) peak is observed. As shown in Fig. 8(a), the maximum g(r) of molecules a, b, c, and d are 0.96, 1.51, 1.40, and 1.48, respectively. These peaks are observed at positions of 5.37, 5.53, 5.09, and 7.49 Å from the Si–H bond, respectively. As shown in Fig. 8(b), the maximum g(r) of molecules a, b, f, and d are found to be 1.78, 1.16, 2.46, and 0.89, respectively. These peaks are observed at positions of 5.01, 9.69, 5.85, and 7.45 Å from the Si–H bond, respectively. Overall, the RDF of system I is smaller than that of system II. The shorter the molecular chain of system I, the higher the vinyl content, and the tighter the molecular configuration of the SRF after crosslinking. The g(r) peak values of the components in the system I are relatively low, the aggregation of molecular chains is stronger, and the distribution of system components is more uniform. These results are consistent with the solubility parameters and Ebinding results.
(8) |
Fig. 9 shows the Rg of the SRF at different vinyl silicone oil viscosities. The Rg value is 12 and 31 Å at viscosities of 0.45 and 200 Pa s, respectively. The structure of system II has a lower aggregation degree. The reason is that vinyl silicone oil has a higher molecular weight and lower vinyl content; therefore, it forms fewer new chemical bonds. This finding is consistent with the RDF results, indicating that the peak value of the RDF is higher in system II.
An increase or decrease in Rg implies disaggregation or aggregation between the molecules, respectively.52 If the molecular aggregates are stable, Rg will be relatively stable. Contrarily, if the molecular aggregates undergo rearrangement or rebonding during the MD simulation, Rg values change over time. Fig. 9 shows Rg values of systems I and II are stable, indicating that the structure did not undergo significant expansion or contraction of during the crosslinking process and confirming its stability during the simulation of components.
σi = Cijεj | (9) |
The stiffness matrix Cij can be obtained from eqn (9) as follows:57,58
(10) |
The elastic constants can be calculated from the stiffness matrix as follows:
λ = ⅙(C12 + C13 + C21 + C23 + C31 + C32) | (11) |
μ = ⅓(C44 + C55 + C66) | (12) |
The mechanical properties parameters such as elastic modulus (E), shear modulus (G), bulk modulus (B), and Poisson's ratio (v) of the system are determined as follows:59–61
(13) |
G = μ | (14) |
B = λ + 2μ/3 | (15) |
(16) |
Table 9 shows the experimental and simulation results of static mechanical properties in systems I and II, with some errors. The values of parameters determined via MD simulations were slightly higher. The errors between the experimental and simulation values were related to the molecular chain length of the polymers. The degree of polymerization of molecules b, c, and f was reduced in the same proportion during the simulation process. The molecules repeat units simulated by molecular dynamics is about 10 times shorter than that of the molecules in the experiment. A shorter the molecular chain implies a higher the vinyl content, and a tighter the molecular configuration of the SRF after crosslinking, leading to higher mechanical properties of the SRF. Thus, the reduction in molecular chain length is the main reason for the higher simulation results of the SRF.
Item | Experimental results | Simulation results | ||||||
---|---|---|---|---|---|---|---|---|
E/MPa | G/MPa | B/MPa | v | E/GPa | G/GPa | B/GPa | v | |
System I | 2.450 | 2.694 | 2.811 | 0.366 | 0.7217 | 0.9512 | 0.6452 | 0.4592 |
System II | 0.997 | 1.370 | 0.663 | 0.247 | 0.6422 | 0.2920 | 0.3575 | 0.4279 |
The changes in the mechanical properties of the SRF with the increasing of the vinyl silicone oil viscosity determined via MD simulation were consistent with those determined experimentally. A comparison of the SRF in systems I and II shows that the static mechanical properties of system II decrease. As the viscosity of vinyl silicone oil increases, the elastic modulus, shear modulus, bulk modulus, and Poisson's ratio of the SRF decrease to ∼59.3%, 49.1%, 76.4%, and 32.5%, respectively, as determined experimentally. These values were determined via MD simulation as ∼11.0%, 69.3%, 44.6% and 6.8%, respectively.
Fig. 10 shows the stress–strain curves of the SRF in systems I and II. The slope value of the elastic stage in the stress–strain curve represents the elastic modulus of each system. System I had a relatively large slope, indicating its higher elastic modulus than system II. This finding is consistent with the results shown in Table 9. These results indicated that changing the vinyl silicone oil viscosity considerably impacted on static mechanical properties of the SRF.
Fig. 11(a)–(d) show the crosslinking density, shore C, tensile strength, and elongation at break of the SRF in systems I and II, respectively. The crosslinking density of the SRF decreases from 4.62 to 4.07 mol mL−1, and shore C decreases from 44.5° to 29°. The tensile strength decreases from 0.86 to 0.61 MPa, whereas the elongation at break increases from 83.4% to 153.5%. As the viscosity of vinyl silicone oil increases, the crosslinking density, shore C, and tensile strength of the SRF decrease, whereas the elongation at break increases. As the viscosity of vinyl silicone oil increases, the length of polymer molecular chains increases and the vinyl content decreases, which loosens the cross-linked network structure of the SRF. The network structure tightens when the vinyl content is high. This indicates that the viscosity of vinyl silicone oil can influence the structure and properties of the SRF. Vinyl silicone oil with a lower viscosity can enhance the crosslinking density of silicone rubber, thereby increasing its tensile strength and hardness. In contrast, vinyl silicone oil with a higher viscosity can impart greater elasticity and longer elongation to silicone rubber. These results were also reported in a previous study.62 Thus, by selecting an appropriate the viscosity of vinyl silicone oil, the SRF with a desired structure and performance can be prepared.
Fig. 11 Mechanical properties of SRF in systems I and II. (a) Crosslinking density; (b) shore C; (c) tensile strength; (d) elongation at break. |
The performance of the SRF cannot be determined solely based on one parameter. For instance, a larger MSD of the system does not necessarily indicate poor performance. A comprehensive analysis must be conducted by considering various parameters such as RDF and δ as well as the application prospects. The cross-linked network structure of the SRF considerably affects the mechanical properties of the SRF. Additionally, the application and requirements of the SRF, such as sealing or cushioning and shock absorption, must be considered to determine its performance.
However, the effect of high-viscosity vinyl silicone oil on the movement of molecular chains and the aggregation degree of molecular structure of the SRF needs futher elucidation. To this end, we noted the following observations. (1) A longer molecular chain implies smaller free volume of the system, the weaker activity of the system's molecular chain, and the lower MSD. (2) System II has a negative Ebinding and lower CED and δ; therefore, its components have poor compatibility. (3) The low vinyl content in the system, fewer crosslinking agents, and low-density network structure increases the Rg. (4) The RDF shows that the aggregation degree of molecular structure in system II is relatively low. Thus, the mechanical property of the SRF is affected by the ability of molecular motion, the size of free volume, multicomponent compatibility, binding energy of the whole system, and the aggregation degree of its molecular chain structure. The mechanical properties of the SRF can be optimized based on the aforementioned parameters.
(1) The polymer molecular chain length is crucial for the SRF performance. As the viscosity of vinyl silicone oil increases, the MSD of the system decreases and Ebinding increases. Meanwhile, the CED and the solubility parameter decrease, leading to poor compatibility between the system components. The aggregation degree weakens with increasing Rg. Thus, the mechanical properties of the system are influenced by the viscosity of vinyl silicone oil.
(2) As the viscosity of vinyl silicone oil increases, the vinyl content decreases, and fewer network structures are formed within the system. The elastic modulus, shear modulus, bulk modulus, and Poisson's ratio of the SRF decrease. The crosslinking density, shore C, and tensile strength of the SRF also decrease, whereas the elongation at break increases. Thus, by selecting an appropriate the viscosity of vinyl silicone oil, the desired performance of SRF can be obtained.
(3) Although some minor differences were observed between the MD simulation and experiment results, they were largely consistent. This provides theoretical support and reference value for the industrial production of the SRF from a microscopic perspective.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d4ra04784b |
This journal is © The Royal Society of Chemistry 2024 |