Deepak
Rase
ab,
Narugopal
Manna
ab,
Rinku
Kushwaha
ab,
Chitvan
Jain
ab,
Himan Dev
Singh
ab,
Pragalbh
Shekhar
ab,
Piyush
Singh
ab,
Yashraj Kumar
Singh
a and
Ramanathan
Vaidhyanathan
*abc
aDepartment of Chemistry, Indian Institute of Science Education and Research, Dr Homi Bhabha Road, Pashan, Pune 411008, India. E-mail: vaidhya@iiserpune.ac.in
bCentre for Energy Science, Indian Institute of Science Education and Research, Dr Homi Bhabha Road, Pashan, Pune 411008, India
cThe Centre of Excellence for Carbon Capture and Removal, Svante Incorporation, 8800 Glenlyon Pkwy, Burnaby, British Columbia V5J 5K3, Canada
First published on 25th March 2024
Quasi-solid-state rechargeable zinc–air batteries (ZABs) are suitable for the generation of portable clean energy due to their high energy and power density, safety, and cost-effectiveness. Compared to the typical alkaline aqueous electrolyte in a ZAB, polymer or gel-based electrolytes can suppress the dissolution of zinc, preventing the precipitation of undesirable irreversible zinc compounds. Their low electronic conductivity minimizes zinc dendrite formation. However, gel electrolytes suffer from capacity fade due to the loss of the volatile solvent, failing to deliver high-energy and high-power ZABs. Consequently, developing polymers with high hydroxide ion conductivity and chemical durability is paramount. We report cationic C–C bonded robust polymers with stoichiometrically controlled mobile hydroxide ions as solid-state hydroxide ion transporters. To boot, we increased the viologen-hydroxide-ion concentration through “by-design” monomers. The polymers constructed with these designer monomers exhibit a commensurate increase in their ionic conductivity. The polymer prepared with 4 OH− ion-containing monomer was superior to the one with 3 OH−. The conductivity increases from 7.30 × 10−4 S cm−1 (30 °C) to 2.96 × 10−3 S cm−1 (30 °C) at 95% RH for IISERP-POF12_OH (2_OH) and IISERP-POF13_OH (3_OH), respectively. A rechargeable ZAB (RZAB) constructed using 3_OH@PVA (polyvinyl alcohol) as the electrolyte membrane and Pt/C + RuO2 catalyst delivers a power density of 158 mW cm−2. In comparison, RZABs with a PVA interlayer provided only 72 mW cm−2. Notably, the device suffered an initial charge–discharge voltage gap of merely 0.55 V at 10 mA cm−2, which increased by only 2 mV after 50 hours of running. The battery operated at 10 mA cm−2 and worked steadily for 67 hours. We accomplished a flexible and rechargeable zinc–air battery (F-RZAB) exhibiting a maximum power density of 79 mW cm−2. This demonstration of a cationic viologen–bakelite polymer-based flexible secondary ZAB with versatile stochiometric hydroxide-ion tunability marks an important achievement in hydroxide-ion conducting solid-state electrolyte development.
Polymeric membranes, which possess an inherent ability to facilitate OH− ion conduction, are commonly referred to as anion exchange polymer electrolyte membranes (AEPEMs). These are distinguished by the presence of positively charged functional groups, such as quaternary nitrogen or imidazole groups and some hydrogen-bonding moieties integrated into the polymer chain.30,34–36 These functional groups play a crucial role in creating interconnected nanochannels and enabling the selective conduction of anions via optimal electrostatic interactions; additionally, they cooperate very well with water within AEPEM networks.37 However, their archetypal 1-D chain structure cannot avoid potential swelling, and if they are electronically conductive, it promotes Zn-dendrimer growth. High structural flexibility and porosity can promote the undesired passage of zincate ions through their pores.38,39 These drawbacks underscore the need for alternative approaches in ZAB design and separator technology. Furthermore, considering that ZABs are designed to be cost-effective energy storage solutions, using expensive commercial AEPEM membranes is not an ideal approach. Consequently, there is a compelling need to engineer cost-effective AEPEMs.
Among polymer electrolytes and gel polymer electrolytes reported, poly(ethylene oxide) (PEO)40,41 or PVDF-based systems,42,43 as well as their combinations with various zinc salts, are the most studied for use in ZABs.44 Polymer electrolytes, such as PEO, show poor ionic conductivity due to their semicrystalline nature. To attain high ionic conductivity, these polymers require the use of organic solvents, such as propylene carbonate (PC), ethylene carbonate (EC), and dimethylsulfoxide (DMSO).42,43,45 Despite having acceptable ionic conductivity, such organic solvents are inapplicable for open systems, such as secondary zinc–air systems, due to their volatility.46 Nevertheless, PVA has proven to be an excellent choice for flexible electrolyte preparation due to its hydrophilic nature and film-forming capabilities.35,47–50 We decided to exploit these advantageous features of PVA by integrating it with a superior hydroxide ion-conducting polymer in an aqueous system.
To this end, robust C–C bonded cross-linked polymers capable of conducting hydroxide ions in humid environments became our target RZAB electrolyte material. Their amorphous nature and low electronic conductivity help minimize zinc-dendrite formation and their microporous structure is expected to favour selective conduction of hydroxide ions, while the organic framework can enable them to be a component of a flexible battery. They generally do not swell under aqueous conditions, hence as solid electrolytes, they will adhere to the electrode as its volume increases or reduces during charging and discharging, respectively.51,52 Thus, in this study, a thin hydroxide ion-conducting solid-state separator coupled with an electrolyte has been devised for use in ZABs by a combination of cationic polymer with PVA through simple solution processing.
Inspired by the versatility of viologen chemistry53,54 earlier we showed how viologen–bakelite polymers can be manipulated to have stoichiometrically loaded mobile hydroxide ions that render them superior quasi-solid electrolytes for primary zinc–air battery.32,33 Following this, with the rapidly surging interest in secondary or rechargeable batteries, we realized the paramount need for demonstrating the potential of this hydroxide ion-conducting cationic polymer in the more challenging target of secondary zinc air battery where its compatibility demands increase.55–57 Specifically, a hydroxide ion-exchanged POF was integrated with PVA to form a solid-state separator-cum-electrolyte for zinc–air battery applications. Moreover, considering that the monomeric building unit of these polymers can be tuned to have a systematically increased number of hydroxide ions per unit, we successfully verified that this stoichiometric control can be translated to enhanced hydroxide ion conductivity. Our demonstration of high-power density and running life for the proposed viologen–bakelite electrolyte-based RZAB creates numerous possibilities.
Scheme 1 Synthetic procedure of 2_OH and 3_OH. Circular insets show the photographic images of compounds 2 and 3. |
There is evidence of Bakelite-type coupling between triazine-resorcinol and viologen-based bipyridinium aldehyde according to analysis of 13C cross-polarisation (CP) magic angle spinning (MAS) solid-state nuclear magnetic resonance (NMR) (Fig. 1a and b). The coupling between an aldehyde and unsubstituted sites on phloroglucinol rings leads to a distinctive aliphatic peak for the C–C bond at 29 and 28 ppm for 2 and 3, respectively. It is followed by other characteristic peaks from aromatic groups, such as triazine, at around 195 ppm for 2 and 191 ppm for 3; aromatic peaks for a viologen-based unit are present at around 142 ppm and 143 ppm for 2 and 3, respectively. The aliphatic peaks for building blocks around 69 ppm and 61 ppm were intact upon the formation of 2 and 3 (Fig. 1a and b).58,59 While this shows that polymerization occurred, we recorded the NMR spectra of the material after boiling it in a THF + DMF mixture and later soaking it over 24 h in a 6 M KOH solution to exchange the Br− with OH− ions. The characteristic peaks were still equally intense and situated at similar chemical shifts. For electrolyte applications, the exceptional chemical stability and functional group integrity of the polymer, especially when subjected to harsh treatments, are highly desirable (Fig. 1a and b). Fig. 1c and d show the comparative FTIR spectrum of aldehyde monomers, i.e., tri and tetra aldehyde, as-synthesized cationic polymers (2 and 3), their hydroxide exchanged forms: 2_OH, and 3_OH. The increase in intensity for C–H (2890 cm−1) clarified that the C–C bond between phenolic and aldehyde moieties had formed, as evidenced by the elimination of CO (1690 cm−1) from the monomers upon polymerization. Additionally, CN (1620 cm−1) ensures the integrity of the building blocks in 2, 2_OH, 3, and 3_OH, respectively (Fig. 1c and d). These are highly cross-linked high-molecular-weight polymers that are insoluble even in boiling solvents (e.g., glycol, DMF, and DMSO); hence, we could not use methods, such as gel permeation chromatography in our characterizations.
Field emission scanning electron microscopy (FESEM) and high-resolution transmission electron microscopy (HRTEM) images of 2 and 3 (Fig. 1e and g) show that polymer particles are agglomerated or intergrown microspheres with sizes ranging from 500 nm to 5 μm (Fig. S1, S3, S6 and S8, ESI†). Fig. 1f and h show that even after treatment of 2 and 3 with a 6 M KOH solution to make 2_OH and 3_OH, respectively, there was no deformation in the shape of these microspheres (Fig. 1f and h and Fig. S2 and S4, ESI†). This shows that their texture remained stable in the corrosive environment. Thus, 2_OH and 3_OH were well suited to operate under highly concentrated alkaline conditions that are necessitated by ZABs. The energy dispersive X-ray (EDX) analysis shows the systematic increment in the atomic percentage of the Br− ions from 1 (ref. 33) to 3. It shows the presence of excess Br− ions available for the exchange with the OH− ions (Fig. S5, ESI†). Moreover, the colour difference in 2 (brown) and 3 (dark brown) echoes the presence of a higher amount of the Br− ions (Scheme 1).
High-resolution transmission electron microscopy (HRTEM) images unveiled that the spherical balls in 2 and 3 (Fig. S6 and S8, ESI†) are connected in a continuous manner, which can support ionic transport across grains and spheres. We noticed no changes in the surface diameter of 2_OH and 3_OH spheres during OH− ion exchange, which further demonstrated the chemical stability of the polymers (Fig. S7 and S9, ESI†). However, the elemental mapping of 2 and 3 (Fig. S6 and S8, ESI†) reveals the presence of the Br− ions, which significantly lowered when exchanged with OH−. The presence of K+ traces demonstrates that the exchange in 2_OH and 3_OH was successful (Fig. S7 and S9, ESI†).
Thermogravimetric analysis displayed that frameworks of 2 and 3 are stable up to 280 °C. We associate this with the strong C–C bond between the monomers, resembling the bonds in Bakelite (Fig. S10, ESI†). The cationic polymers treated with 6 M KOH, i.e., 2_OH and 3_OH, display similar TGA profiles (Fig. S10, ESI†) and exhibit no effect of harsh alkaline conditions on their thermal stabilities.
The contact angle measurements on the surface of freshly synthesized halogen-containing polymer powders, labelled as 2 and 3, indicated a super-hydrophobic nature (Fig. S11, ESI†). However, 2_OH and 3_OH prepared by exchanging the halogen for hydroxide ions in an aqueous alkaline medium resulted in hydrophilic powders (Fig. S12, ESI†). This change in surface wettability positively influences the interaction of materials with electrolytes. We investigated molecular porosity using water sorption isotherms. The water adsorption isotherms for 2, 3, 2_OH, and 3_OH were almost identical, indicating that the pore environment and structure had not undergone significant changes; however, the water capacity of 2_OH and 3_OH was higher than that of 2 and 3, demonstrating the improved intrinsic wettability of the former. Thus, materials with Br− containing frameworks are nearly super-hydrophobic (140 ± 3°) and become significantly hydrophilic when bromides are replaced by the OH− ions (Fig. S13a, ESI†). Notably, neither a significant change in density nor a detectable swelling of the polymer occurred (Fig. S13b–f, ESI†).
The equivalent circuit was fitted for all Nyquist curves using the Zview-4 software. The comparison of the most promising Nyquist plots (30 °C, 95% RH) for 2_OHvs.3_OH (Fig. 2a) suggests that the series and charge-transfer resistance types are substantially higher for 2_OH (R1 = 140.1 Ω, R2 = 281.3 Ω) compared to 3_OH (R1 = 35.4 Ω, R2 = 61.6 Ω). However, 2_OH and 3_OH exhibit typical semi-infinite linear diffusion, i.e., diffusion in one dimension that is only constrained by a substantial planar electrode on one side (at a 45° angle to the z′-axis). We confirmed the need for a CPE component by measuring the CV of 2_OH and 3_OH, which showed that the capacitive behaviour was present in the fitted equivalent circuit (Fig. S15c and S18, ESI†). A pseudocapacitive behaviour anticipated for the polymer with the porous structure is shown by a CPE-P value close to 0.5 for both pellets. In our scenario, hydroxide ions move through pathways created by the presence of hydroxyl groups and triazine. These pathways can potentially facilitate the formation of hydrogen bonds, contributing to the Grotthuss mechanism. However, concurrently applying an AC potential can generate sufficient force to induce vehicular motion.
Furthermore, we investigated AC-impedance by varying the temperature (30 °C to 80 °C) to examine the humidity-dependent conductivity of 2_OH and 3_OH (Fig. 2b, S16 and S17, ESI†). Comparative heatmaps of 2_OH and 3_OH show that conductivities of the polymers range from 10−8 S cm−1 (30% RH at 30 °C) to 10−2 S cm−1 (95% RH at 80 °C). A steady rise in conductivity values was seen up to 80% RH as the temperature was elevated, but after that, both the polymers exhibited a sudden increase in conductivity (where the area on the plot changes from green to yellowish orange). Particularly, 3_OH has a higher conductivity value than 2_OH even at lower temperatures, especially above 80% RH (the wider area covered by the red-coloured zone).
Increasing hydroxide ion conductivity with increasing temperature implies a lowering of the activation energy. In contrast, increased conductivity with increasing humidity means that water could play a crucial role via hydrogen bonding. This takes into account the fact that the polymer lacks a crystalline structure with well-organized pores and that its electronic conductivity is constrained at longer-length scales.60 To examine the electronic conductivity of 2_OH and 3_OH, linear sweep voltammetry (LSV) was used at a scan rate of 10 mV s−1 across a potential window of −1 to 1 V (Fig. S19, ESI†). The conductivity observed for 2_OH and 3_OH is primarily ionic, likely due to the OH− ions, as evidenced by their minimal electronic conductivity.
Activation energies of 0.49 eV and 0.45 eV for 2_OH and 3_OH are obtained when the Arrhenius equation is fitted to temperature-dependent impedance data (Fig. 2c), which points to the occurrence of the Grotthuss diffusion process.61 The reported activation energy for hydroxide ions in various nano-porous materials is comparable to observed activation energies.62
It must be noted that when comparing our results to those of earlier research, the polymers show a gradual increase in hydroxide ion conductivity from 1_OH33 to 3_OH (Fig. 2d and Table S1, ESI†)., which was anticipated, given the systematic increment in intrinsic hydroxide ion concentrations. The activation energy obtained from 1_OH to 3_OH is almost the same since the structural environments of the polymers remain similar among all three cases. Using the Z′ vs. ω−1/2 plot, we computed the diffusion coefficient for hydroxide ions inside the cationic polymer framework. The low-frequency spectrum in the impedance plot produced distinctive linear fits (Fig. S20, ESI†) from which the diffusion coefficients at 80 °C and 95% relative humidity were calculated to be 3.61 × 10−5 cm2 s−1 (2_OH) and 3.71 × 10−5 cm2 s−1 (3_OH). As the temperature rose, the diffusion coefficient increased systematically (Fig. S20, ESI†). The calculated diffusion coefficients at 80 °C and 95% relative humidity agreed well with values published in the earlier publication 2.9 × 10−5 cm2 s−1 (1_OH).
The best-performing polymer, i.e., 3_OH, was tested for temperature-dependent cycling stability in an 8 hours cycle ranging between 30 °C and 60 °C at 95% relative humidity (Fig. 2e). The cycling demonstrated excellent conductivity retention when temperature was varied between 30 °C and 60 °C. We also measured conductivity for various batches of 3_OH, and the results are in the same order (Fig. 2f inset-top). Additionally, for more than 50 hours, outstanding time-dependent stability of up to 95% was demonstrated for conductivity (Fig. 2f inset-bottom). Regarding post-impedance characterization, the polymers 2_OH and 3_OH showed excellent chemical and structural integrity. The SS-NMR demonstrates retention of all peaks from pristine polymers (Fig. S21, ESI†), and the surface morphology is also intact in FESEM images (Fig. S22 and S23, ESI†).
The remarkable robust nature of the polymers makes them apt candidates for charge storage applications in harsh alkaline conditions like zinc–air batteries. We explored the application potential of exceptional hydroxide ion-conducting viologen polymer 3_OH as a solid-state electrolyte in a zinc–air battery. A thin, flexible, and stable membrane is developed by blending 3_OH and polyvinyl alcohol (PVA) in a 1:1 ratio (3_OH@PVA), as shown in Fig. 3a. Photographs shown in red circles are images of the membrane at different stages. According to the FESEM images (Fig. 3a, highlighted in a yellow ring, and Fig. S24a, ESI†), membranes with a uniform surface would considerably assist in creating an interface between the electrode and electrolyte. The ultra-thin membrane with a thickness of just 277 μm is seen in the cross-sectional FESEM images. It contains uniformly distributed polymer spheres, which assist in speeding up ion transport via a shorter path (Fig. S24d and e, ESI†). The analysis of AFM images and amplitude roughness parameters indicates that the electrolyte membrane exhibits satisfactory flatness. The consistent mean surface roughness (Sa) values, ranging from 177 nm to 268 nm across different samples, demonstrate that the membrane maintains a consistent level of flatness (Fig. S25 and Table S2, ESI†). Measurements of the conductivity of the membrane revealed a significantly promising hydroxide ion conductivity of 4.78 × 10−3 S cm−1 at room temperature (25 °C) in the presence of 95% humidity. The conductivity increased, reaching a maximum of 2.53 × 10−2 S cm−1, when the temperature was changed from room temperature to 80 °C (Fig. 3b). Along with superior ionic conductivity, the membrane exhibits excellent flexibility on bending, stretching and crumbling (Fig. 3c–f). Minimal change in membrane thickness was observed, when the membrane was immersed in an alkali solution for 12 hours indicating excellent stability in alkaline conditions (Table S3, ESI†).
The performance of the system is comparable to previously reported ZAB systems in the literature (refer to Table S4, ESI†). The comparative analysis of steady-state cell polarization (Fig. 4c) reveals maximum power densities (Pmax) of 72 mW cm−2 and 158 mW cm−2 for ZABs utilizing PVA and 3_OH@PVA as membranes, respectively. Notably, the 3_OH@PVA-based cell gradually improved its performance compared to the PVA-based counterpart, ultimately it outperformed the latter. This improvement can be attributed to the intrinsic advantages of 3_OH@PVA membranes, particularly in terms of mass transport facilitated by the membrane and interface formation between the electrolytes. Furthermore, the superior performance of the 3_OH@PVA membrane can be directly attributed to the improved ionic conductivity of the membrane an enhanced contact achieved at the electrode–electrolyte interface.
To determine the specific capacities of the prepared ZAB cell, the discharge process was carried out to a voltage of 1.38 V at a current density of 10 mA cm−2. Moreover, the galvanostatic discharge curve, captured at a current density of 10 mA cm−2 (Fig. 4d), provides evidence of the durability of the ZAB system. It is noteworthy that discharge durations for ZABs utilizing 3_OH@PVA and PVA as membranes are approximately 22 hours and 8 hours, respectively (Fig. 4d inset). The observed voltage decreases within the plateau region over the course of operation, which is likely attributable to side reactions occurring at the surface of the zinc powder, as indicated in prior studies. The calculated specific capacity, as illustrated in Fig. 4d, for the constructed zinc–air battery (ZAB) utilizing 3_OH@PVA membrane as the separator-cum-electrolyte, amounts to approximately 742 mA h gZn−1. In comparison, the ZAB system employing PVA as the separator-cum-electrolyte exhibits a specific capacity of around 579 mA h gZn−1. The failure of RZAB (PVA-KOH) systems after 8 hours can be attributed to the rapid drying of the commercial and PVA-KOH membranes within the semi-open ZAB system configured for air-breathing. This drying phenomenon is a consequence of inferior electrolyte retention characteristics exhibited by the PVA-KOH membrane.
Furthermore, Fig. 4e displays galvanostatic charge–discharge curves recorded for cells operating at 10 mA cm−2. The zinc–air battery (ZAB) fabrication using 3_OH@PVA revealed a lower voltage difference (0.55 V) between charging and discharging compared to PVA-KOH (0.72 V). Over 67 hours of continuous charge–discharge cycles, the 3_OH@PVA membrane-based cell showed a nominal increase of 0.02 V in the voltage difference. In contrast, the PVA-KOH-based system exhibited a rapid increase to 0.67 V within just 17 hours, leading to the termination of the test. Additionally, the inset image (Fig. 4e) of the magnified charge–discharge profile between 14 to 18 hours shows the symmetric plateau nature of the 3_OH@PVA membrane-based RZAB, while the PVA-KOH cell displayed asymmetric behaviour. This difference reveals the better interface formation and water uptake capacity of 3_OH@PVA compared to PVA-KOH which helps run charge–discharge devices for long durations.
In response to the growing interest in portable and flexible electronic devices, we designed and demonstrated a flexible and rechargeable zinc–air battery (F-RZAB) with a surface area of 2 × 2 cm2. This innovative system utilized a catalyst-coated carbon cloth as the cathode, a 3_OH@PVA-based membrane as the electrolyte, and a polished 0.10 mm thick zinc foil as the anode (Fig. 5a). A flexible solid-state ZAB was developed to demonstrate the practical usability of the as-prepared 3_OH@PVA (Fig. 5a), resulting in a combined voltage of 1.386 V, as measured using a multimeter device (Fig. 5b). More information is provided in the ESI Section.† Without additional O2 gas purging, the constructed solid-state battery delivers an OCV value of 1.38 V (Fig. 5b) in air. According to the polarisation study shown in Fig. 5c, the maximum power density was 79 mW cm−2. The output voltage remained stable on bending the device at different angles (Fig. 5d–g), owing to the liquid-free nature of 3_OH@PVA.
The flexibility of the device was assessed by monitoring its open-circuit voltage (OCV) at various bending angles (0°, 90°, and 180°). Remarkably, the system maintained a consistent OCV of approximately 1.40 V across these different bending angles (Fig. 5d). Fig. 5e–g shows the digital photographs of the flexible device from various angles.
The neat PVA membrane displayed a few tiny fractures during battery measurements (Fig. S28b–d, ESI†). In contrast, the membrane in the case of 3_OH@PVA is stable and undamaged with uniformly distributed spherical polymer particles (Fig. S29e and f, ESI†), just like initial condition of the membrane (Fig. S24a, ESI†). Additionally, the thickness of 3_OH@PVA dropped from 277 μm to 177 μm (Fig. S28d, ESI†) on post-battery characterization, which may be attributed to pressure applied during battery packing.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d4sc00121d |
This journal is © The Royal Society of Chemistry 2024 |