First published on 22nd December 2023
A one-step thermal polymerization approach was adopted to combine C3N5 with montmorillonite nanosheets (MMT Ns) to form xCN-MMT for the degradation of pollutants in water. Benefitting from the abundant hydroxyl groups on the MMT surfaces, double defects (–CN and N defects) were introduced in xCN-MMT catalysts to promote the adsorption of tetracycline (TC), peroxymonosulfate (PMS), and oxygen. 10CN-MMT exhibited superior adsorption performance toward TC, with the adsorption capacity being 5.65-fold that of MMT Ns and 2.64-fold that of C3N5. Further, 10CN-MMT exhibited better PMS activation performance than MMT Ns and C3N5, which could degrade 95% of TC within 120 min. Moreover, the total organic carbon (TOC) removal efficiency of the present system reached 81.1%, and the chemical oxygen demand (COD) decreased from 50.7 to 12.2 mg L−1. The degradation process of TC was characterized using liquid chromatography-tandem mass spectrometry (LC-MS), and a reasonable degradation pathway and catalytic mechanism were given by combining with active species analysis. The toxicological analysis of the degradation products also showed a significant decrease in toxicity. The degradation experiments in different water environments were also simulated, and it was found that 10CN-MMT showed good adsorption effects. This study provides a green metal-free clay-based catalyst and shows good applicability in removing antibiotics.
Environmental significanceTetracycline (TC) has become the most commonly used antibiotics due to its low cost, wide range of applications, and multiple modes of intake. However, TC causes environmental damage when it enters the ecosystem and cannot be effectively removed by traditional water treatment methods due to its stable structure. Activated peroxymonosulfate (PMS) is a typical advanced oxidation process (AOP) that generates reactive radicals (·OH and SO4˙−) by transition metal ions, UV light, heat, and electrochemical processes. However, these methods may lead to the leaching of metal ions and consume large amounts of energy, which results in secondary water pollution. Therefore, we used a one-step thermal polymerization method to combine C3N5 with montmorillonite nanosheets (MMT Ns) to form xCN-MMT for the degradation of pollutants in water. 10CN-MMT was able to degrade 95% of TC within 120 min through the synergistic effect of adsorption and degradation. In the 10CN-MMT/PMS system, the total organic carbon (TOC) could reach 81.1%, and the chemical oxygen demand (COD) was reduced from 50.7 mg L−1 to 12.2 mg L−1. Therefore, this study not only provides a new idea for the construction of metal-free clay-based catalysts but also provides a green and efficient catalyst for the activation of PMS to degrade antibiotics. |
Carbon nitride is a typical metal-free material with high thermal stability, non-toxicity, low cost, and unique electronic properties, which can replace metal-based catalysts for environmental treatment. Carbon nitride with nitrogen functionalities (e.g., –NH2, –NH–) serves as strong Lewis base sites, which are potential ideal sites for metal-based catalysts.8 Guan et al.9 prepared a variety of C3N4 using different precursors with different catalytic activities for PMS activation, which could remove BPA with 100% efficiency within 15 min. Different preparation processes affect the chemical composition and structure of the catalysts, thus changing the type of active sites. In addition, it has been demonstrated that the nitrogen content can be adjusted to achieve efficient environmental purification and energy conversion.10 Kumar and coworkers11 synthesized a novel N-rich polymer carbon nitride material with a stoichiometric ratio of C:N = 3:5 (C3N5). Unlike the structure of g-C3N4 in which three heptazine units are linked to the tertiary nitrogen, the two s-heptazine units in the C3N5 polymer are linked together by an azo bond, constituting an utterly new bonding mode.12 Porous C3N5 exhibited excellent adsorption performance for methylene blue11 and the adsorption process reached 90% adsorption–desorption equilibrium within only 1 min, achieving adsorption–desorption equilibrium within 10 min. Fu et al.13 prepared piezoelectric-photocatalysts C3N5-x-CN for the removal of tetracycline. This catalyst demonstrated excellent efficiency toward tetracycline removal, with a kinetic constant of 0.0342 min−1, which can be further improved in the presence of PMS. The double-defective sites in the catalyst synergistically greatly improved the catalytic activity. These results indicate that C3N5 acts as a promising candidate in various applications, especially in the field of wastewater treatment. However, the activation of PMS by C3N5 alone without the aid of additional energy still faces the problem of low activity, so further modification of C3N5 is needed to improve its catalytic properties.
Montmorillonite (MMT) is a typical water-bearing layered silicate clay mineral and shows strong hydrophilicity due to high charge density on the lamellar surface.14,15 Thus, MMT can be easily exfoliated into montmorillonite nanosheets (MMT Ns) under external forces characterized by small size, high surface energy, and strong dispersion. In addition, montmorillonite has abundant hydroxyl groups on its surface, and these properties make MMT show great potential in the design and synthesis of novel mineral functional materials.16,17 Surface hydroxyl groups can not only help to immobilize other nanomaterials to form heterojunctions and improve the mass transfer rate between PMS and contaminants but can also be used to construct defective sites in the composites. Liu et al.18 used MMT as a support material to anchor CoxMn3−xO4 nanoparticles, and the composites showed excellent ability to activate PMS. Zhang et al. utilized the abundance of coal gangue surface hydroxyl groups introduced in C3N4 with double nitrogen defects, which could remove 90% of BPA after activation of PMS within 30 min.19 Inspired by previous excellent works, the introduction of C3N5 in MMT Ns is likely to show efficient PMS activation performance for the degradation of pollutants in water.
Hence, a series of metal-free catalysts (xCN-MMT) based on MMT and C3N5 was prepared for the purpose of efficient PMS activation to degrade TC without the help of additional energy. The catalysts were comprehensively analysed, experimental parameters were optimized, and the reaction mechanism and possible degradation pathways of TC were proposed. This work constructed a novel reaction system for activating PMS without metal catalysts, which provides a new idea for purifying water resources.
(1) |
(2) |
The degradation intermediates of TC were analysed using the liquid chromatography-quadrupole time-of-flight mass spectrometer (LC-Q-TOF-MS), which was equipped with Thermo Fisher. A total organic carbon (TOC) analyser (Shimadzu TOC, Japan) was used to analyse the mineralization efficiency. A chemical oxygen demand (COD) analyser (CBPN-401C/D, COD, Guangzhou) used a closed digestion colorimetric method to measure the amount of organic matter in water.
The FT-IR spectra of MMT, C3N5, and 10CN-MMT are shown in Fig. 1c. In the spectrum of C3N5, the peak located at 3167 cm−1 is attributed to the surface residual –NH2 and/or –OH stretching. The peaks at 1641, 1462, 1413, 1323, and 1245 cm−1 are related to the triazine ring stretch. The peaks at 885 and 808 cm−1 are ascribed to the bending vibrations of N–H. These results are in good agreement with previous reports.22,23 The absorption peak at 3628 cm−1 is attributed to the hydroxyl stretching vibration of structural water in the MMT lattice. In the spectrum of MMT Ns, the absorption peak at 3440 cm−1 belonged to the hydroxyl stretching vibration of adsorbed water in the MMT interlayer. The absorption peak at 1641 cm−1 is the hydroxyl bending vibration of adsorbed water molecules. The broad absorption peak at 1029 cm−1 corresponds to the Si–O–Si stretching vibrations in the MMT lattice. The weak absorption peak at 910 cm−1 belongs to the bending vibration of the octahedral hydroxyl group in MMT.24,25 The spectra of 10CN-MMT showed the characteristic peaks of both C3N5 and MMT, indicating the co-presence of C3N5 and MMT. A new vibration peak at 2192 cm−1 is observed for 10CN-MMT, being attributed to the cyano group (–CN),19,26 suggesting that the –CN group was introduced during the thermal polymerization process in the presence of MMT. Furthermore, the FT-IR spectra of all xCN-MMT samples and the effect of the MMT hydroxyl group were investigated. As shown in Fig. 1d, all xCN-MMTs catalysts exhibit similar FT-IR spectra with a distinct –CN peak at 2192 cm−1. In order to further investigate the role of hydroxyl groups on the MMT surface, MMT was calcined at different temperatures and used to synthesize CN-MMT catalysts. As shown in Fig. 1e, the characteristic peaks of hydroxyl groups on the MMT surface at 3628 and 3440 cm−1 disappeared after calcination at 700 and 800 °C, indicating that the surface hydroxyl groups were removed. Interestingly, the –CN of 10CN-MMT (700 °C) and 10CN-MMT (800 °C) catalysts also disappeared (Fig. 1f). The results further indicated that the MMT surface hydroxyl groups have an important effect on the generation of –CN groups in the catalysts.
The chemical composition and surface characteristics of C3N5, MMT Ns, and 10CN-MMT were investigated by XPS measurement. As shown in Fig. 2a, the XPS spectra of C3N5 contained predominantly C, N, and a small amount of O, which could be attributed to atmospheric moisture or CO2 adsorbed on the C3N5 surface.21 The signals of Al, Si, C, N, and O elements were all observed in the full survey XPS spectra of 10CN-MMT. As shown in Fig. S1,† the characteristic peaks of Al 2p and Si 2p orbitals were shifted from 75.98 and 104.1 eV in MMT Ns to 76.15 and 104.2 eV in 10CN-MMT, respectively. It is well known that the electronegativity of an atom affects the electron density around it. The decrease in electron density reduced the electron shielding effect and thus enhanced the binding energy.27 The electronegativity of C and N atoms differed from that of Si and Al atoms. Thus, the strong interfacial interactions upon the binding of MMT Ns and C3N5 shift the characteristic peaks toward higher binding energies.28
Fig. 2 The full survey XPS spectra (a), N 1s spectra (b), and C 1s spectra (c) of C3N5 and 10CN-MMT. |
The high-solution C 1s XPS spectra of C3N5 and 10CN-MMT are displayed in Fig. 2c. In the C 1s spectrum of C3N5, four peaks located at 285.4, 286.5, 288.6, and 289.6 eV were attributed to indeterminate carbon (C1), C–NHx group (C2), carbon atoms bonded by the three N-adjacent bonds (C3) and C–NH2 groups (C4), respectively.29 As for the C 1s spectra of 10CN-MMT, it is seen that the proportion of C3 peaks was significantly reduced, which indicated that the N2–CN– structure at the tertiary carbon position was disrupted, and more defects were formed.30 Meanwhile, the intensity of the C1 peak significantly increased, indicating that more indeterminate carbon was formed, possibly due to the formation of N defects.
As shown in Fig. 2b, the peaks in the N 1s spectra located at 399.3 eV (N1) and 400.8 eV (N2) were attributed to CN–C group nitrogen atoms and bridging nitrogen atoms (C–NN–C) or amino nitrogen atoms (C–NH2), indicating the presence of triazine and triazole groups in all C3N5-based materials. However, in the 10CN-MMT sample, a significant weakening of the N 1s signal is observed, which might be related to the presence of N defects. Besides the decrease in the N1 peak intensity, the peak intensity ratio of N1/N2 simultaneously decreased from 1.68 for C3N5 to 1.03 for 10CN-MMT, suggesting that the defects in the sample might have eliminated part of the triazine structure.29 The introduction of MMT Ns led to defective sites of C3N5, mainly originating from the triazine ring position. To further demonstrate the formation of N defects, elemental analysis was performed on 10CN-MMT (Table S1†). In 10CN-MMT, the C/N atomic ratio was 1.16, indicating a significant decrease in N content, which confirmed the loss of lattice nitrogen and the creation of nitrogen defects in the catalyst.19
The presence of N-defects was further verified using ESR measurements (Fig. S2†). The Lorentz line with a g value of 2.003 indicated the unpaired electrons of the C atoms in the aromatic ring, which originate from the redistribution of the remaining electrons in the nitrogen loss.31 The 10CN-MMT sample exhibited a strong symmetry signal at g = 2.003 in comparison with pristine C3N5. Thus, the reaction between the hydroxyl group on the MMT surface and the 3-amino-1,2,4-triazole intermediate during the complexation process introduced the N defects (N-d) and –CN group into C3N5. The introduction of defects promoted the electron transfer ability and reduced the reaction energy barrier for the adsorption of pollutants and PMS molecules.7 In addition, as a typical strong electron acceptor, the –CN group had strong electrophilic properties that could promote electron redistribution.32 These properties strongly influenced the subsequent adsorption and degradation performance.
In order to obtain detailed morphological information on C3N5, MMT Ns, and 10CN-MMT, the TEM technique was performed. As shown in Fig. 3a, the synthesized C3N5 displayed the morphology of fragmented agglomerates. MMT nanosheets showed a completely clear film-like morphology (Fig. 3b). TEM images of 10CN-MMT (Fig. 3c) showed that the C3N5 fragments were in close contact with the MMT Ns and dispersed uniformly. Fig. 3d shows the HRTEM images of the composites, and no apparent lattice fringes were found. EDS elemental mapping (Fig. 3e) shows that the C, N, Al, and Si elements in 10CN-MMT are uniformly distributed. In addition, the presence of MMT Ns induces a more dispersed feature of C3N5, which is conducive to improving the adsorption capability.
Fig. 3 TEM images of C3N5 (a), MMT Ns (b) and 10CN-MMT (c). HRTEM images (d) and EDS element mapping (e) of Al, Si, C, and N for 10CN-MMT. |
The effect of other parameters on the adsorption performance was also evaluated. Fig. S4b† shows the effect of 10CN-MMT dosage on the adsorption efficiency. The adsorption efficiency improved from 32% to 66% with a continuously increased adsorbent dosage. This phenomenon indicated that the increase in the sample concentration could provide a large number of adsorption sites, which was beneficial to increase the contact between the sample and the pollutant, thus improving the adsorption performance of the sample. Fig. S4c† showed the effect of initial TC concentration on adsorption efficiency. The results showed that good adsorption efficiencies were exhibited for different concentrations of TC, with 10CN-MMT adsorbing 66% of the TC within 60 min at a TC concentration of 50 mg L−1. Fig. S4d† shows the effect of temperature on the adsorption efficiency of 10CN-MMT on TC. As the temperature was increased from 0 °C to 55 °C, the adsorption efficiency was almost unchanged, indicating that the temperature had no significant effect on the TC adsorption performance. For energy saving, 25 °C was chosen as the rational temperature.
It is well known that pH value is one of the most critical parameters affecting TC adsorption efficiency and adsorbent surface charge. Thus, a series of adsorption experiments with different pH values were carried out (Fig. S4e†). The adsorption efficiency could adsorb almost 100% of TC at pH = 1–3. When the pH value was adjusted to 11, the adsorbent had almost no adsorption performance, which indicated that the alkaline condition was not favourable for the removal of TC. This result might be related to the fact that the molecular morphology of TC changes at different pH ranges (Fig. S4f†), which includes cationic species (pH < 3.3), zwitterionic species (3.3 < pH < 7.7), and anionic species (pH > 7.7).33,34 The increase in adsorption efficiency at a pH lower than 3.3 was attributed to electrostatic adsorption between the negatively charged catalyst surface and the TC cationic species. When the pH value was above 7.7, the adsorption competition between OH− and TC anionic species and the electrostatic repulsion between the negatively charged catalyst surface and the anionic TC appeared, which resulted in poor adsorption efficiency. As for the pH values between 3.3 and 7.7, the TC molecules as zwitterions were adsorbed on the sample surface by electrostatic interaction, the adsorption competition and electrostatic repulsion were weakened, and the adsorption capacity and adsorption efficiency were increased. Based on the above discussion, a pH value of 5 was chosen as the optimum condition for the following experiments.
Pseudo-first-order model:
qt = qe(1 − exp(−k1t)) | (3) |
Pseudo-second-order model:
(4) |
Webber–Morris model:
qt = kid × t1/2 + C | (5) |
Elovich model:
(6) |
Kinetic data for the adsorption of TC over C3N5, MMT Ns, and 10CN-MMT are presented in Fig. 5 and Table S2.† As displayed in Table S2,† the pseudo-second-order and Elovich models matched well with the adsorption data, which indicated that the adsorption process of TC over C3N5, MMT Ns, and 10CN-MMT was more suitable for the pseudo-second-order and Elovich models. It also confirmed the inhomogeneous adsorption and interaction between TC molecules and C3N5, MMT Ns, and 10CN-MMT.38 The adsorption capacity of 10CN-MMT (44.8 mg g−1) was much more significant than those of MMT Ns (7.93 mg g−1) and C3N5 (16.9 mg g−1) in the pseudo-second-order kinetic adsorption model, indicating the significant role of MMT in enhancing the adsorption performance of C3N5.
Fig. 5 Pseudo-first-order (a), pseudo-second-order (b), Webber–Morris (c), and Elovich (d) models for adsorption of TC over various adsorbents. |
The adsorption isotherm models could be used to study the interaction between pollutants and adsorbents at equilibrium and the distribution of adsorbed molecules at the solid–liquid interface during adsorption. Four isothermal adsorption models were chosen to fit the adsorption process of 10CN-MMT. Freundlich isothermal adsorption model: commonly used to describe the adsorption of a multimolecular layer occurring on an inhomogeneous surface, where the adsorption occurs at different locations with different adsorption energies;39 Langmuir isothermal adsorption model: assumed that monolayer adsorption occurs on the surface of the adsorbent; Temkin isothermal model: describes the adsorbent during the adsorption of a solute, where the interaction of adsorbates generate the heat of adsorption; the Redlich–Peterson isothermal model is a combination of the Freundlich and Langmuir models.40,41
Langmuir model:
(7) |
Freundlich model:
(8) |
Temkin model:
qe = Aln(KTCe) | (9) |
Redlich–Peterson model:
(10) |
The data of the four adsorption models corresponding to the adsorption process of TC by adsorbent 10CN-MMT are shown in Fig. S5† and Table S3.† The fitting coefficient of Langmuir and Redlich–Peterson isothermal models, R2 = 0.997, is higher than that of Freundlich (R2 = 0.897) and Temkin (R2 = 0.972) isothermal models. The fitting coefficients of 10CN-MMT indicate that the adsorption process of TC by 10CN-MMT is suitable for the Langmuir and Redlich–Peterson isothermal model, i.e., TC molecules belong to the adsorption mode of the co-existence of monolayer adsorption and multilayer adsorption on the adsorbent 10CN-MMT.
SO4˙− + HSO5− → SO5˙− + SO4− + H+ | (11) |
·OH + SO4˙− → HSO5− | (12) |
SO4˙− + SO4˙− → S2O82− | (13) |
·OH + ·OH → H2O2 | (14) |
Fig. 6 Effects of CN loading amount (a), catalyst dosage (b), TC concentration (c), PMS concentration (d), temperature (e) and pH value (f) on the catalytic efficiency. |
Fig. 6e shows the effect of temperature on the efficiency of TC degradation by 10CN-MMT-activated PMS. As the temperature was increased from 0 °C to 55 °C, the degradation efficiency increased slightly, indicating that the temperature had a slight effect on the TC degradation performance. The initial pH also significantly influences the activation of PMS for TC degradation. As shown in Fig. 6f, 10CN-MMT could effectively degrade TC at different pH values. When the initial pH was increased to 13, the degradation efficiency could reach 66% even though the adsorption efficiency decreased, ascribed to the consumption of ·OH, thus impeding the generation of active species (eqn (15)–(17)).43
OH− + HSO5− → SO52− + H2O2 | (15) |
OH− + SO4˙− → SO42− + ·OH | (16) |
·OH + SO52− → SO5˙− + OH− | (17) |
Based on the above discussion, it was concluded that the maximum adsorption capacity was 44.8 mg g−1 and the maximum efficiency of activated PMS for TC degradation was 95% of sample 10CN-MMT at pH = 5, initial TC concentration = 50 mg L−1, temperature = 25 °C, PMS concentration = 0.3 mmol L−1, and catalyst dosage = 0.8 g L−1.
The Chemical Oxygen Demand (COD) values after adsorption and degradation of TC by 10CN-MMT were tested under optimal catalytic conditions (Fig. 7a).44 The COD values in the solution showed a significant decrease after the adsorption and degradation process, indicating a significant reduction of organic matter in the system. The total organic carbon (TOC) value of the system was tested and used to evaluate its mineralization efficiency (Fig. 7b). The TOC value of 10CN-MMT was 81.1% within 120 min when the initial TC concentration was 50 mg L−1, indicating that most TC molecules had been converted to CO2 and H2O. Table S4† summarizes the comparison of the catalytic activity of 10CN-MMT with other reported metal-free catalysts for activating PMS to degrade pollutants in water, demonstrating that 10CN-MMT is a promising catalyst for activating PMS to remove pollutants, and it could achieve a high level of mineralization efficiency for TC. Combined with FT-IR analyses (Fig. 7c), it was found that adsorption and degradation reactions occurred on the 10CN-MMT surface. Although the positions of the vibrational peaks did not change significantly after adsorption and degradation, the vibrational peaks around 2192 cm−1 almost disappeared after degradation. This phenomenon indicated that the –CN group played a crucial role in the activation process of PMS and participated in the activation process. Because MMT surface hydroxyl groups can be removed by calcination above 700 °C, MMT was calcined at 700 and 800 °C to obtain hydroxyl-free MMT, and subsequent samples of 10CN-MMT (700, 800 °C) were prepared. The catalytic performance of 10CN-MMT (700, 800 °C) was significantly inhibited in comparison to the 10CN-MMT catalyst (Fig. S8a†). Thus, –CN group played a critical role in PMS activation. However, the characteristic peak of –CN in 10CN-MMT reappeared after treatment with alkali heat conditions, which implies that the activity could be restored by alkali heat method. To verify this result, the cycling experiment was performed (Fig. S8b†). 10CN-MMT exhibited a slight decrease in degradation efficiency after 5 cycles, which indicated that the catalyst 10CN-MMT had excellent recyclability. Fig. S8c† shows the XRD pattern of the 10CN-MMT after-reaction and alkaline-heated samples. The crystallinity of the sample decreased after the reaction but improved significantly after alkaline heat treatment. Thus, the decrease in the intensity of the vibrational peak at 2192 cm−1 of the alkaline-heated sample was the main reason for the decrease in the catalytic performance. Since the –CN group played a critical role in PMS activation, the reduction of –CN might affect the catalytic reactivity and cause a decrease in TC degradation efficiency.
The groundwater usually contains many different anions, such as Cl−, H2PO4−, HCO3−, and SO42−, which also could scavenge free radicals in the process of AOPs. Thus, the effect of different anions on the removal of TC by 10CN-MMT was investigated (Fig. 7d). SO42−, Cl−, and NO3− slightly affected the adsorption efficiency, which might be due to competitive adsorption with TC molecules. On the other hand, H2PO4− was more ionized than hydrolysed, generating more H+ and contributing to a lower solution pH, which made adsorption more likely to occur. The ability of HCO3− to bind hydrogen ions was more significant than its ability to ionize hydrogen ions, so the solution was alkaline and inhibited the adsorption of TC by 10CN-MMT. In addition, HCO3− could also react with SO4˙− or ·OH to form CO3˙− with lower oxidation capacity (eqn (18) and (19)).5
·OH + HCO3− → H2O + CO3˙− | (18) |
SO4˙− + HCO3− → SO42− + H+ + CO3˙− | (19) |
In addition, various metal ions and macromolecular organics were present in the wastewater, Ca2+ and Na+ as metal ions, and humic acid (HA) as macromolecular organics were selected to evaluate the pollutant removal ability of 10CN-MMT. As shown in Fig. 7e, when the ion concentration was increased from 0 to 0.01 mol L−1, the adsorption performance of 10CN-MMT was almost unaffected by Na+ and Ca2+ and only slightly decreased. The reason could be attributed to the fact that the presence of Ca2+ and Na+ would occupy the active sites of the adsorbent, leading to adsorption competition between TC molecules and metal ions. Besides, the presence of metal ions might affect the surface charge of 10CN-MMT, which weakened the interaction between TC molecules and adsorbent, resulting in electrostatic repulsion.39 The influence of Ca2+ in these two aspects was more significant than that of Na+, so the presence of Ca2+ had a more significant effect on the adsorption performance of 10CN-MMT. Fig. 7f shows the effect of different concentrations of humic acid (HA) on TC adsorption efficiency. The adsorption and degradation efficiencies were hardly affected when humic acid concentration was increased from 0 to 20 mg L−1.
To investigate the general applicability of the 10CN-MMT catalyst further, different water sources and various pollutants were selected as degradation targets. Deionized water, tap water, river water (Dahei River, Hohhot), reclaimed water (Xiaohei River, Hohhot), and lake water (Nan Lake, Hohhot) were chosen to simulate the aqueous environment in real applications (Fig. S9a†). The results showed that the 10CN-MMT catalyst could effectively degrade TC in different water environments at a low catalyst dosage. The pH test of different water samples displayed neutrality. Thus, the improved performance might be related to the presence of various ions in the solution. This result indicated that the synthesized catalysts were highly adaptable. As shown in Fig. S9b,† the degradation efficiencies of 10CN-MMT for 2,4-p-nitrophenol (2,4-DCP), ciprofloxacin (CIP), and oxytetracycline (OTC) in the range of 50 mg L−1 were 45%, 99%, and 84%, respectively. The results showed that 10CN-MMT exhibited significant removal effects for phenolic compounds and antibiotics, especially antibiotics that could achieve high removal efficiencies. Thus, it had good applicability in removing various pollutants.
The mutagenicity value, acute toxicity LC50 of fathead minnow, and acute toxicity LC50 of Daphnia magna of TC and its intermediate products were analysed by employing the Toxicity Estimation Software Tool (T.E.S.T.) according to quantitative structure–activity relation (QSAR) prediction (Fig. S11†).48,49 According to the prediction in Fig. S11a,† some of the intermediates were still positive for mutagenicity, but the mutagenicity values of the final products were mostly reduced to negative. The LC50 (LC50 after 96 h) of TC for Fathead minnow was 0.9 mg L−1, implying that TC was very toxic. Most of the degradation products had higher LC50s, reflecting that the acute toxicity of the TC solution was significantly reduced by degradation (Fig. S11b†). Similarly, in Fig. S11c,† the LC50s of almost all intermediates for Daphnia magna were lower than that of TC (5.44 mg L−1) except P5, P1, and P4, indicating that the toxicity of the TC solution has been dramatically reduced after degradation. The above toxicity prediction results indicated that the 10CN-MMT catalyst could effectively degrade TC and reduce the overall toxicity of TC during PMS activation.
ESR analysis was conducted to demonstrate further the active species produced during the activation of PMS by 10CN-MMT. As shown in Fig. S12,† no peaks were observed in the PMS system with the addition of DMPO and TEMP, which meant that PMS could not produce the active species alone without a catalyst. As shown in Fig. 9b–d, the 10CN-MMT and 10CN-MMT/PMS systems were compared. The catalyst alone could also not produce active species to degrade the pollutants and thus adsorb the pollutants. However, after using 10CN-MMT to activate PMS, distinct characteristic peaks appeared. It proved that active species ·OH, SO4˙−, 1O2, and O2˙− were present in the 10CN-MMT system. In addition, ·OH might be converted to SO4˙− and thus not easily quenched by TBA.52,53
Based on the reported studies and the above analysis of active species, the proposed mechanism for the study of TC removal by 10CN-MMT activated PMS is shown in Fig. 10 and eqn (20)–(28) as follows.
C–π + HSO5− → C–π+ + OH− + SO4˙− | (20) |
C–π + HSO5− → C–π+ → H+ + SO5˙− | (21) |
2SO5˙− → 2SO4˙− + O2 | (22) |
SO4˙− + H2O → SO42− + ·OH + H+ | (23) |
2·OH + 2HSO5− → 2SO4˙− + O2 + 2H2O | (24) |
2SO5˙− + H2O → 2HSO4− + 1.51O2 | (25) |
–CN/Nd + O2 → 1O2 | (26) |
O2 + e− → O2˙− | (27) |
TC + SO4˙−/·OH/O2˙−/1O2 → intermediates → CO2 + H2O | (28) |
Footnote |
† Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d3va00331k |
This journal is © The Royal Society of Chemistry 2024 |