Vijay
Tripathi‡
a,
Siddarth
Jain‡
*a,
Dinesh
Kabra
b,
Leela S.
Panchakarla§
a and
Arnab
Dutta
*acd
aDepartment of Chemistry, Indian Institute of Technology Bombay, Mumbai, 400076, India. E-mail: arnab.dutta@iitb.ac.in; jainsiddarth477@gmail.com
bDepartment of Physics, Indian Institute of Technology Bombay, Mumbai, 400076, India
cInterdisciplinary Program in Climate Studies, Indian Institute of Technology Bombay, Mumbai, 400076, India
dNational Center of Excellence in CCU, Indian Institute of Technology Bombay, Mumbai, 400076, India
First published on 25th November 2022
Strategically doped metal oxide nanomaterials signify a rapidly growing genre of functional materials with a wide range of practical applications. Copper vanadate (CuV) represents one such highly active system, which has been rarely explored following its doping with an abundant first-row transition metal. Here, we have developed a series of CuV samples with varying cobalt(II) doping concentrations deploying a relatively simple solid state synthetic procedure. Among the samples, the 10% Co(II)-doped CuV (Co10%–CuV) exhibited excellent reactivity for both the H2 evolution reaction (HER) and glycerol oxidation reaction (GOR) in an alkaline aqueous medium (pH 14.0) during cathodic and anodic scans, respectively. During this dual-active catalysis, surface-immobilized Co10%–CuV operates at exceptionally low overpotentials of 176 mV and 160 mV for the HER and GOR, respectively, while achieving 10 mA cm2 current density. The detailed spectroscopic analysis revealed the formation of formate as the major product during the GOR with a faradaic efficiency of >90%. Therefore, this Co10%–CuV can be included on either side of a two-electrode electrolyzer assembly to trigger a complete biomass-driven H2 production, establishing an ideal carbon-neutral energy harvest process.
Metal oxides can be constituted of multiple components present in either stoichiometric or non-stoichiometric amounts, harbouring several cations in divergent coordination geometries. Therefore, metal oxide templates can support the facile transformation of different metal oxidation states, which is vital for creating reaction hot spots on the surface of the material leading to unique electrocatalytic capabilities. Metal vanadate is an exciting class of metal oxides that can generate numerous reactive states to be useful for direct applications in the fields of electrocatalysis, photocatalysis, energy storage systems, magnetic devices, etc.15–19 Copper vanadates are one of the top choices in this regard, which can exist in variable conformations, such as CuV2O6, Cu2V2O7, Cu3V2O8, Cu11V6O26, and Cu5V2O10 while displaying a range of p and n-type semiconductor phases.20–24 Copper vanadates have gained attention due to their structural versatility (nanostructure or film) and tunable electrochemical and photocatalytic properties. The strategic alterations of reaction temperature, synthesis method, reactants, and other reaction conditions minutely tune the different phases of these particular vanadates. The critically developed CuV2O6 nanoparticles and nanobelts have found their usage as electrode materials in batteries.21,22 On the other hand, Cu3V2O8 was employed for photocatalysis and water splitting.23 Cu5V2O10 contains distorted Cu(II) ions, which were instrumental in showcasing unique magnetic anisotropy.24 Nickel vanadate (Ni3V2O8) was doped with Co(II) to craft CoNi2V2O8 that can be potentially implemented as an electrode material for batteries and supercapacitors;25 whereas tungsten or molybdenum doping in bismuth vanadate leads to its improved and efficient performance as a photo-electrode and in electrochemical applications.26 Cu2V2O7 has also been substantially investigated as a photo-anode material, while its transition metal doped counterparts such as Co–Mg doped and Zn doped Cu2V2O7 have demonstrated multiferroic and dielectric properties.27,28 Cu2V2O7 was also doped with the divalent 3d-transition metals Zn(II) and Mn(II) to further explore their prospective applications in photocatalysis. Despite the commendable progress in this realm, the specific influence of doped copper vanadates is mostly restricted to photoanode, supercapacitor, battery, and photocatalyst-based applications.29–33 The potential of these otherwise unusual materials has been rarely probed for electrochemical reductions (cathodic) and organic molecule oxidations.
The current energy scenario and the negative impacts of excessive fossil fuel usage have exacerbated environmental pollution challenges and compelled human society to explore alternative solutions leading to sustainable development. The utilization of renewable energy and biomass has been reckoned to be one of the best options in pursuing a carbon-neutral energy landscape. The storage of intermittent renewables into a chemical vector H2 is a key step, where the presence of a hydrogen evolution reaction (HER) catalyst is essential. On the other hand, a catalyst capable of oxidizing the reduced carbon sources and extracting the stored energy is vital for harnessing biomass energy. However, copper vanadates have rarely been probed as electrocatalysts for the electrocatalytic HER and organic molecule oxidation reactions. However, copper vanadate provides a robust and conductive template, which can be activated with strategic doping with appropriate materials. In this regard, cobalt ions offer an excellent option. The widely abundant and inexpensive cobalt ions are well-known for their role in supporting electrocatalytic water-splitting reactions. Recent research reveals that the electrocatalytic efficacy of the HER is enhanced by the presence of cobalt ions owing to the favourable hydrogen adsorption energy of their interfacial cobalt sites (compared to those of other 3d metals such as Ni and Fe). Additionally, cobalt ions also promote water adsorption and dissociation on the catalyst surface to drive the water oxidation reaction.34,35 Similarly, the role of cobalt-based catalysts in promoting glycerol oxidation into various value-added products (C1–C3) has been explored lately.36,37
Here, in this work, we have rationally incorporated a Co(II) dopant in a copper vanadate (Cu2V2O7) framework to explore its capability of driving both the HER and glycerol (a reduced carbon resource) oxidation (Scheme 1). The 10% cobalt doped electrocatalyst was screened to be the optimized electrocatalyst that demonstrated excellent HER (overpotential 176 mV @ 10 mA cm−2) as well as glycerol oxidation (overpotential 160 mV @ 10 mA cm−2) in an alkaline aqueous solution (pH = 14). During the oxidation reaction, formic acid was found to be the major product, which is reckoned as a crucial C1 feedstock in the chemical industry. Therefore, developing this new class of dual-active electrocatalysts can establish a solid foundation for designing devices capable of simultaneously generating fuel and processing biomass.
The structural configuration of pure CuV and Co(II)-doped CuV (Co0–20%–CuV) were investigated further using SEM (Fig. S2a–d†). The morphology of pure copper vanadates (Co0%–CuV) revealed the existence of agglomerated nanoparticles in clusters with an average diameter of 30–40 nm, indicating a homogeneous growth of nanoparticles (Fig. S2a†). SEM images obtained from Co(II) samples displayed no significant change in particle size or morphology, showcasing the conservation of the same copper vanadate framework (Fig. S2b–d†).
Next, the morphology of the model Co(II)-doped sample (Co10%–CuV) was studied by TEM analysis, which reaffirmed the formation of 30–40 nm diameter nanoparticle formation (Fig. 1b). HR-TEM was employed to gain a better insight into the Co10%–CuV structure. The lattice fringes of Co10%–CuV revealed a highly crystalline phase with a d-spacing of 0.26 nm, inferring growth along the (220) plane (Fig. 1c). In addition, there are no secondary structures or impurities evident in the image, indicating that all Co(II) ions are uniformly integrated into the copper vanadate template without any cobalt clustering. The TEM-EDS data confirmed the uniform distribution of Co, Cu, V, and O elements in the copper vanadate matrix (Fig. 1d and S3†). The dopant concentration in the copper vanadate matrix was precisely measured using inductively coupled plasma-atomic emission spectroscopy (ICP-AES), where the Co10%–CuV sample registered 9.6% doping of cobalt ions.
The X-ray photoelectron spectroscopy (XPS) experiment was performed on the Co10%–CuV sample next to probe the chemical environment of each element. The full scan XPS spectrum reiterated the presence of all the precursor elements in the matrix with the signature Co 2p, Cu 2p, V 2p, and O 1s peaks (Fig. S4†). The Co 2p3/2 and Co 2p1/2 signals of the sample were observed at 782 and 798 eV, respectively. The occurrence of this 16 eV difference between Co 2p3/2 and Co 2p1/2 suggests that dopant cobalt ions primarily exist in the sample in the Co(II) oxidation state.6,38 These signals were also accompanied by the higher energy shakeup satellites (2p3/2, 785.1 eV and 2p1/2, 802 eV) (Fig. 2a). The oxidation state of Cu in the Co10%–CuV host lattice was also validated using XPS data. The high-resolution XPS spectrum of the Cu 2p region exhibits prominent peaks positioned at 934.9 (Cu 2p3/2) and 955.2 eV (Cu 2p1/2), which can be ascribed to the presence of Cu(II) ions (Fig. 2b). The satellite peaks located at 942.9 and 962.6 eV indicate an open 3d9 shell in the structure.39,40 Furthermore, shoulder peaks at lower binding energies were also noticed for both the Cu 2p3/2 and Cu 2p1/2 signals. These peaks may be attributed to reduced Cu(I) sites, which were probably generated to compensate for the oxygen vacancies present in the copper vanadate framework.41 The existence of the V(V) chemical state in the matrix of Co10%–CuV was verified by the primary V 2p asymmetric peaks with binding energies of 524.9 (V 2p3/2) and 517.4 eV (V p1/2) (Fig. 2c).39 The O 1s region comprises three components: a small peak at around 529.8 eV owing to oxygen and defects and two wider peaks at 531.7 and 533.4 eV originating from lattice oxygen Cu–O and V–O respectively (Fig. 2d).42,43
Fig. 2 High resolution XPS spectra of (a) Co 2p, (b) Cu 2p (c) V 2p and (d) O 1s regions of the 10% Co(II)-doped Cu2V2O7 (Co10%–CuV) sample prepared at 550 °C under an inert atmosphere. |
(i) Volmer–Heyrovsky mechanism:
H2O + e− + M* ↔ MH* + OH− (Volmer reaction, b ∼ 120 mV dec−1): H2O dissociation |
MH* + H2O + e− ↔ H2 + M + OH− (Heyrovsky reaction, b ∼ 40 mV dec−1): H desorption |
(ii) Volmer–Tafel mechanism:
H2O + e− + M* ↔ MH* + OH− (Volmer reaction): H2O dissociation |
MH* + MH* ↔ H2 + 2M (Tafel reaction b ∼ 30 mV dec−1): H recombination |
The Tafel slope will be ∼120, ∼40, or ∼30 mV dec−1 if the rate-determining step is a Volmer, Heyrovsky, or Tafel reaction, respectively.50 This catalyst also showcased the most facile kinetics which was corroborated by the corresponding Tafel slope. The Tafel slopes for Co0%–CuV, Co5%–CuV, Co10%–CuV, and Co20%–CuV are found to be 145 mV dec−1, 113 mV dec−1, 94 mV dec−1, and 120 mV dec−1, respectively (Fig. 3b). Throughout this investigation, the Tafel slopes have been found to be greater than 40 mV dec−1, demonstrating that the HER is governed by the Volmer–Heyrovsky mechanism. Next, the bulk electrolysis (chronocoulometry) experiment was performed with the Co10%–CuV sample (immobilized on a carbon paper working electrode) in an air-tight cell while maintaining a constant applied potential of −0.2 V. The head-space gas was collected periodically during this experiment and analyzed via a gas chromatography (GC) instrument. The GC data confirmed the evolution of H2 during the reduction (Fig. 3c and 4d). This data also indicated an excellent faradaic efficiency (FE) of 93.7% by Co10%–CuV during the electrocatalytic HER. The electrocatalytic HER activity showcased by Co10%–CuV matched the proficiency of state-of-the-art H2 production catalysts in alkaline media in terms of applied overpotential (η @ 10 mA cm−2) and kinetics (Table S1†). Comparative LSV data were also collected with the same Co10%–CuV electrode following bulk electrolysis (at −0.2 V), which matched the pre-electrolysis HER response (Fig. S5a†). The long-term electrochemical durability of the Co10%–CuV modified electrode, which demonstrated a high HER performance, was further examined via chronoamperometry (j vs. t measurement). Fig. S5b† shows long-term chronoamperometry stability (up to 4 h, at a constant bias of −0.2 V) without current density decay, validating electrochemical endurance under practical conditions.
The Co(II) dopant tends to replace the Cu(II) from the host copper vanadate lattice. This ion replacement creates a disparity in the original skeletal structure and leads to oxygen vacancies to balance the overall charge of the lattice. These induced vacancies presumably produce active sites for enhanced electrocatalytic activity. Furthermore, to understand the significance of cobalt doping in enhancing the intrinsic electrocatalytic activity of Co10%–CuV for the HER, we studied the link between the Co ions and electrochemical kinetics (EIS study), as well as the active electrochemical surface area (ECSA) of the catalyst during the HER. As shown in Fig. 3e, electrochemical impedance spectroscopy (EIS) measurements were undertaken. As depicted in Fig. 3e (inset), the charge transfer resistance (Rct) and solution resistance (Rs) are determined by fitting the plots using a simplified Randles circuit model. 10% Co(II) doped CuV has a significantly lower Rct (37) than the 5% Co(II) doped CuV (52) pure CuV (70), indicating faster charge transfer via the catalytic electrode and, consequently, a rapid reaction rate in electrocatalytic kinetics. This also indicates the strong conductivity of the Co(II) doped CuV modified electrode, which speeds up reactions and hence decreases the HER overpotential. The solution resistance (Rs) has a specific value of around 14.7 ohm. The effective ECSA of the pure CuV and doped CuV samples was estimated by calculating the double-layer capacitance (Cdl), which is a typical way to measure the interfacial area between the electrolyte and electrode surface, recording to the CV curves at various scan rates.51,52 The current density vs. scan rate graphs in Fig. S6† show that 10% Co(II) doped CuV has a Cdl value of 1.9 mF cm−2, which is greater than that of 5% Co(II) doped CuV (0.95 mF cm−2) and undoped CuV (0.5 mF cm−2) and suggests that 10% Co doped CuV has a higher ECSA and a greater number of active sites for the HER. The effect of cobalt doping on electrocatalytic performance was also validated by an optical band gap study (Tauc-plot) of Co0%–CuV (2.5 eV), Co5%–CuV (2.13 eV), and Co10%–CuV (2.05 eV) respectively (Fig. S7†). The presence of Co(II) ions significantly lowered the band gap of the pure Co0%–CuV (2.5 eV), as the 5% and 10% cobalt-doped samples illustrated 2.13 and 2.05 eV band gaps, respectively. Therefore, a specific amount of Co doping drops the band gap and surface electronic structure of doped copper vanadates implying an improved electrical contact and lowered electric resistance, which enhances the charge transfer kinetics to boost the heterogeneous HER.34,35,53
We also evaluated the ECSA normalized activity and turn over frequency (TOF) in order to examine the intrinsic catalytic GOR activity of the cobalt-doped CuV electrocatalysts. The results are shown in Fig. S10 and S11.† The CuV with 10% Co(II) doping has the highest values. After normalizing the GOR LSV polarization curves using their respective ECSAs (Fig. S10†), 10% Co(II) doped hybrids show the lowest onset potential and a greater current density than the undoped copper vanadate, showing that Co10%–CuV has the best electrocatalytic performance per active unit for the GOR process compared to the undoped sample. Turnover frequency (TOF) may indeed be utilised to assess the intrinsic activity of electrocatalysts with more precision when their active sites are well identified. Previous experiments have clearly shown that Co(II) ions play a crucial role in facilitating the Co(II) doped CuV sample to carry out the GOR electrocatalysis. While identifying the active sites in single-element catalysts is relatively straightforward, multi-element composite catalysts provide unique challenges due to a lack of comprehensive techniques and understanding of catalytic mechanisms. A generally established strategy is to assume all metal sites to be active, despite the fact that this would result in an underestimation of the TOF. The TOF values (at 1.6 V vs. RHE) of catalysts were computed and compared as shown in Fig. S11† based on the number of active sites (postulating Co combined with Cu and V) determined by ICP-AES. Co10%–CuV reveals a much larger TOF in comparison to undoped copper vanadate, similarly to the ECSA-normalized current density. These findings indicated that Co10%–CuV has a higher innate activity toward the GOR compared to other composites.
1H nuclear magnetic resonance (1H NMR) spectroscopy was deployed to identify the glycerol oxidation products following bulk electrolysis of Co(II)-doped copper vanadate. In this experiment, relatively modest potentials of 1.6 and 1.7 V were applied to limit the interference from the competitive OER. Formic acid is identified as the primary product of the Co10%–CuV-catalyzed GOR, as evident from the comparative 1H NMR spectra recorded before and after the electrolysis (Fig. 4d and e). The 1H NMR peak of formic acid was standardized further to determine the faradaic efficiency (FE) of the electrocatalytic GOR (Fig. S12†). This investigation confirmed the generation of formic acid with an FE of 79.8% at 1.6 V, which is comparable to that in previously reported work (Table S2†).55 The 13C NMR analysis was executed following the bulk electrolysis to further verify the glycerol oxidation products. The formate ions emerged as one of the major products, along with substantial amounts of carbonate (Fig. S13†). The 1H NMR spectra illustrated the presence of glyceric acid, lactic acid, and acetic acid, albeit at lower amounts compared to formate (Fig. 4e). These intermediate products provide us hints to decipher the glycerol oxidation mechanism, which is addressed in the subsequent segment. The applied potential has a direct effect on the product selectivity, as the FE for formic acid dropped on either side of 1.6 V (the applied potential) (Fig. 4f). The lack of available energy typically slows down the GOR at 1.5 V, while at 1.7 V, the competitive OER kicks in.
Scheme 2 depicts a probable route for the electrochemical oxidation of glycerol to formate in an alkaline solution based on experimental findings and earlier reports.48 Electron-rich glycerol initially oxidizes to glyceraldehyde following a two-electron oxidation triggered by the Co(II)-doped copper vanadate. The highly reactive glyceraldehyde readily converts to glycerate. The formation of glycerate during the reaction was corroborated by 1H NMR spectroscopy (Fig. 4e). This glycerate intermediate undergoes a C–C cleavage, followed by a two-electron transfer, resulting in the formation of equal quantities of formate and glycolate. The electron-rich glycolate continues on the oxidative track to generate another molecule of formate. The glycerol to formate oxidation can also follow an alternative pathway, where glyceraldehyde serially converts to dihydroxyacetone, pyruvaldehyde, 2-hydroxypropenal, lactic acid, and finally acetic acid. The possible presence of this minor oxidation pathway was indicated by the signature 1H NMR signals of acetate and lactate (Fig. 4e). Hence, Co10%–CuV represents one of the leading GOR electrocatalysts showcasing excellent product selectivity and energy efficiency.
Long-term stability of the catalysts under electrocatalytic conditions is a key factor for developing practical assemblies with a higher technology readiness level (TRL). For the lifetime measurement of the Co10%–CuV electrode, an 8 hour long continuous chronocoulometry experiment was performed at an applied potential of 1.6 V. During the experiment the current response changes up to (∼30%) over the course of the experiment (Fig. S14†). Comparative LSV data were also recorded with the same Co10%–CuV electrode post chronocoulometry, where the electrocatalytic GOR activity was retained by the electrode (Fig. S15†). To probe the repeatability of the bulk GOR activity, the Co10%–CuV modified electrode was deployed for electrocatalytic glycerol oxidation for five continuous cycles of bulk electrolysis (applied potential 1.6 V, duration 1 hour). Impressively, the Co10%–CuV electrode continued to oxidize glycerol with minimal loss (<5%) during this experiment (Fig. S16†). Therefore, this Co10%–CuV sample demonstrates the potential of direct inclusion for practical devices driving both the electrocatalytic HER and GOR.
Footnotes |
† Electronic supplementary information (ESI) available: Experimental details, XRD data of the Cox%–CuV nanostructure, Tauc-plot, EIS spectrum, amperometric data, 1H NMR, additional LSV data, and comparison data of electrical performance in tabular form. See DOI: https://doi.org/10.1039/d2na00724j |
‡ These two authors contributed equally. |
§ Chemistry Department, Indian Institute of Technology Bombay, Mumbai 400076, India; (deceased). |
This journal is © The Royal Society of Chemistry 2023 |