Angus
Pedersen‡
abc,
Kavita
Kumar‡
d,
Yu-Ping
Ku
de,
Vincent
Martin
c,
Laetitia
Dubau
c,
Keyla Teixeira
Santos
c,
Jesús
Barrio
ab,
Viktoriia A.
Saveleva
f,
Pieter
Glatzel
f,
Vinod K.
Paidi
f,
Xiaoyan
Li
g,
Andreas
Hutzler
d,
Maria-Magdalena
Titirici
b,
Antoine
Bonnefont
c,
Serhiy
Cherevko
d,
Ifan E. L.
Stephens
*a and
Frédéric
Maillard
*c
aImperial College London, Department of Materials, Royal School of Mines, London SW7 2AZ, UK. E-mail: i.stephens@imperial.ac.uk
bImperial College London, Department of Chemical Engineering, London SW7 2AZ, UK
cUniv. Grenoble Alpes, Univ. Savoie-Mont-Blanc, CNRS, Grenoble-INP, LEPMI, 38000 Grenoble, France. E-mail: frederic.maillard@grenoble-inp.fr
dForschungszentrum Jülich GmbH, Helmholtz-Institute Erlangen-Nürnberg for Renewable Energy (HI ERN), Cauerstraße 1, 91058 Erlangen, Germany
eFriedrich-Alexander-Universität Erlangen-Nürnberg, Department of Chemical and Biological Engineering, Cauerstraße 1, 91058 Erlangen, Germany
fESRF, The European Synchrotron, 71 Avenue des Martyrs, CS40220, 38043 Grenoble Cedex 9, France
gLaboratoire de Physique des Solides CNRS, Université Paris Sud, 91405 Orsay, France
First published on 30th July 2024
Atomic Fe in N-doped C (Fe–N–C) catalysts provide the most promising non-precious metal O2 reduction activity at the cathodes of proton exchange membrane fuel cells. However, one of the biggest remaining challenges to address towards their implementation in fuel cells is their limited durability. Fe demetallation has been suggested as the primary initial degradation mechanism. However, the fate of Fe under different operating conditions varies. Here, we monitor operando Fe dissolution of a highly porous and >50% FeNx electrochemical utilization Fe–N–C catalyst in 0.1 M HClO4, under O2 and Ar at different temperatures, in both flow cell and gas diffusion electrode (GDE) half-cell coupled to inductively coupled plasma mass spectrometry (ICP-MS). By combining these results with pre- and post-mortem analyses, we demonstrate that in the absence of oxygen, Fe cations diffuse away within the liquid phase. Conversely, at −15 mA cm−2geo and more negative O2 reduction currents, the Fe cations reprecipitate as Fe-oxides. We support our conclusions with a microkinetic model, revealing that the local pH in the catalyst layer predominantly accounts for the observed trend. Even at a moderate O2 reduction current density of −15 mA cm−2geo at 25 °C, a significant H+ consumption and therefore pH increase (pH = 8–9) within the bulk Fe–N–C layer facilitate precipitation of Fe cations. This work provides a unified view on the Fe dissolution degradation mechanism for a model Fe–N–C in both high-throughput flow cell and practical operating GDE conditions, underscoring the crucial role of local pH in regulating the stability of the active sites.
Broader contextLow-temperature proton exchange membrane fuel cells (PEMFC) fuelled by green hydrogen offer the potential for providing decarbonized energy. Platinum (Pt) is commonly used as a electrocatalyst, but due to its rarity and cost, minimizing its loading is crucial for widespread technology deployment. Atomically-dispersed iron atoms coordinated to nitrogen-doped carbon (Fe–N–C) are primary contenders to replace Pt as electrocatalysts for the O2 reduction reaction. While researchers have made huge inroads towards reaching parity between the two classes of catalysts in terms of activity, the durability of Fe–N–C falls far short of that of Pt. Our current study demonstrates that, at relevant current densities for PEMFC applications, iron atoms dissolve and then reprecipitate in the form of iron oxides. This outcome is a result of an increase in local pH, i.e. across the electrode | electrolyte interface, as indicated by results from online inductively coupled plasma mass spectrometry and a microkinetic model specifically developed for this study. Even at a moderate O2 reduction current density of −15 mA cm−2geo at 20 °C, the local pH rises from 1 to 8–9. Given that practical electrochemical energy conversion and storage systems operate at significantly higher current densities, we expect substantial variations in pH in real fuel cells and water electrolyser devices. These pH changes will affect reaction kinetics, selectivity, and durability. Consequently, ensuring the alignment of local pH with bulk pH emerges as a crucial, albeit underexplored, factor for the sustainable operation of energy storage and conversion systems. |
However, Fe–N–C durability is still below commercial realization for transport applications (>5000 h)17 owing to several degradation routes,18 which can be separated into two categories. Firstly, support modification, such as oxidation of the N–C matrix,2,19,20 and N-protonation (especially for materials synthesized through pyrolysis under ammonia).21 Second is direct active metal atom modification by agglomeration/aggregation, and demetallation/dissolution.19,22,23 The demetallation of the active site can also take place indirectly through chemical or electrochemical corrosion of the N–C matrix.24 Steps can be taken to deconvolute these degradation pathways25 and also minimize them,26,27 or even temporarily reverse them by reactivation.28 However, studies point towards the demetallation of FeNx active sites being the primary irreversible performance degradation mechanism in PEMFCs6,29,30 and the first step in the aggregation scenario.22
Inductively coupled plasma mass spectrometry (ICP-MS) is a highly sensitive technique which can provide time- and potential-resolved Fe dissolution profiles from Fe–N–C catalysts. Monitoring Fe dissolution from ex situ ICP-MS, in tandem with other characterization techniques, in rotating disc electrode (RDE)31 and PEMFC has revealed significant dissolution of Fe,32 although probing the mechanism requires operando measurements. In the first online flow cell ICP-MS study, Choi et al. suggested formation of insoluble ferric (Fe3+) species, which dissolve under PEMFC operating conditions (Ecathode < 0.7 VRHE) due to operando reduction to soluble ferrous (Fe2+) cations.27 This is in line with former ex situ ICP-MS findings of Zelenay and coworkers31 who suggested higher solubility of Fe2+ species in acid solutions compared to Fe3+ species. Previous online flow cell ICP-MS studies also provided critical information on the effects of pyrolysis atmosphere, bulk electrolyte pH, and catalyst modification on the extent of Fe dissolution.19,27,33
Nonetheless, flow cell ICP-MS studies are limited to low current densities, and cannot reproduce all the practical conditions occurring in an operating PEMFC device (O2 partial pressure and current density, lower relative humidity).34 In this respect, online gas diffusion electrode (GDE) ICP-MS is an adequate tool to simulate the environment of a PEMFC cathode more realistically, and gain PEMFC-relevant durability trends. For instance, Ehelebe et al. first demonstrated significantly lower dissolution of Pt/C catalysts in GDE configuration compared to flow cell systems due to varying mass transport conditions of Pt species,35 as previously proposed.36 Very recently, Choi and coworkers26 monitored in situ changes in active site density and operando Fe dissolution of a Fe–N–C under Ar and O2 at different temperatures using GDE ICP-MS cell in acidic conditions. From site density monitoring, the reduced turnover frequency confirmed a reactive oxygen species catalyzed carbon corrosion scenario.24,37 However, despite using a GDE, Choi and coworkers current densities at 0.6 V chronoamperometric holds (<10 mA cm−2geo) were comparable to values achievable in flow cell (∼1–2 mA cm−2geo), and not practical PEMFCs. They observed from post-mortem transmission electron microscopy (TEM) and energy dispersive X-ray spectroscopy (EDXS) elemental mapping that Fe deposited as FexOy nanoparticles after O2 reduction in their Fe–N–C derived from microporous zeolitic imidazolate framework-8 (ZIF-8), confirming earlier findings from Kumar et al.37 Evidence of FexOy nanoparticle formation in PEMFC-relevant conditions has previously been ascribed to highly active but unstable high-spin FeN4C12 moieties, via Mössbauer spectroscopy.38
Temperature is also a critical parameter for durability of Fe–N–C catalysts. Goellner et al. first evidenced that the rate of corrosion of a N–C matrix (150 square wave cycling between 0.9–1.4 VRHE, 3 s holds in RDE) increases 14-fold when temperatures increase from 20 to 80 °C. This resulted in 18-fold larger O2 reduction activity decay (at 0.8 VRHE), which was assigned to N–C corrosion.39 Carbon corrosion can be avoided at 25 °C in RDE by keeping potential <0.9 VRHE,19 although some carbon corrosion (<7 mA cm−2geo) is reported in PEMFC at 80 °C.23 Kumar et al. reported Fe cluster formation under load cycling (Ar-saturated 0.1 M H2SO4, 0.6–1.0 VRHE) at 80 °C, but did not observe Fe clusters at 60 °C, providing strong evidence of the effect of temperature on the fate of Fe species.22 Finally, we note that Osmieri et al. reported greater performance loss under air-fed vs. N2-fed PEMFC cathode (3 s holds at 0.95 and 0.6 Vvsanode, 80 °C), although with no nanoparticle formation.40 Meanwhile Banham et al. qualitatively proposed a larger reaction zone in the Fe–N–C catalyst layer under air vs. O2 due to the difference in O2 concentration and also improved stability with lower equivalent ionomer due to improve ionic conductance.41 Therefore, conflicting characterisation results in literature could be due to operation conditions, (temperature, gas atmosphere, ionomer content and type, current densities, potential etc.), storage conditions,42 electrode preparation43 and synthesized Fe–N–C properties.38 Moreover, most of Fe–N–C catalysts studied by operando ICP-MS have consisted of low active site utilization Fe–N–C derived from ZIF-8. Our laboratory,44 and others,45,46 have highlighted that such catalysts display a predominantly or purely microporous structure. This limits the mass transport and electrochemical active site utilization (number of electrochemically accessible FeNx sites to the total number of FeNx sites) to typically <10%.44–46 This prompted us to revisit Fe dissolution and the fate of Fe in FeNx active sites from our recently developed high FeNx utilisation (>50%) Fe–N–C with high micro- and meso-porosity.44 This pore structure can facilitate mass transport of reactants for improved activity, while also enabling transport of dissolved Fe ions for operando ICP-MS detection.
The impact on Fe–N–C activity from changes in the (micro-) environment from RDE to GDE/PEMFC has been discussed.47–49 Local pH is one value which could vary between electrocatalysts and testing conditions, and is recognized to influence Fe–N–C activity.50–52 Meanwhile, the influence of pH on degradation is beginning to receive greater attention in modelling reaction mechanisms and dissolution trends.53 Local pH (at the interface between the working electrode and the bulk of the electrolyte) and its effects has been investigated and discussed quite extensively in electrochemical CO2 reduction;54,55 however, so far it has garnered limited experimental and theoretical evidence for ORR.56–58 This is because experimental pH probes (scanning probe, laser, RRDE, Raman, IR)59 have been limited to detecting proton concentrations away from the catalyst layer, are limited in pH ranges, cannot be easily transferred to high current devices such as GDEs and in some cases requires the addition of additives. Very recently Sauvé and coworkers proposed a new potential decay electrochemical technique for measuring pH within catalyst layers.60 Still, their method is restricted to providing an average interfacial pH of the electrode, relies on the H2/H+ equilibrium on Pt, and has an overestimation of the pH swing.
Meanwhile, kinetic modelling work by Zenyuk and Litster found during ORR increased pH along Pt mesopore channels, when devoid of Nafion and instead filled with water.61 It is worth considering that FeNx active sites are proposed to be located within micropores,23,45,62 which are expected to be filled with water.23 Even so, Banham and coworkers’ experiments suggest that micropore flooding does not contribute significantly to PEMFC performance decay.63 Instead, kinetic models of Fe–N–C activity decay under different potentiostatic conditions in PEMFCs have been previously proposed,23,64,65 which has led to some debate.66,67 Still, to date these kinetic models of Fe–N–C have not factored in pH change and conditions in GDEs have not been considered.
In this work, we monitored Fe dissolution of a high electrochemical utilization Fe–N–C catalyst using operando flow cell and GDE ICP-MS. We found that the fate of Fe–N–C catalysts is determined by combined Fe demetallation, reactive oxygen species action (magnifying Fe demetallation) and local pH changes caused by ORR. We used a suite of complimentary pre- and post-mortem characterization techniques (SEM, TEM, STEM, EDXS, EELS, Raman spectroscopy, XRD, XPS, XANES) to illustrate changes in structure and chemistry; based on our experimental insights, we built a microkinetic modelling to interpret our observations.
(i) The ORR kinetics in the GDE is limited by proton mass transport, with the O2 concentration being uniform in the catalyst layer.
(ii) The dissolution and precipitation of Fe cations occurs in the water present in the pores i.e., the precipitation of Fe cations is not influenced by the Nafion ionomer in the catalyst layer:
Fe3+ + 3H2O → Fe(OH)3 + 3H+ |
(iii) Due to the pronounced difference in complexation constants, only Fe3+ cations are expected to precipitate.71 If Fe2+ cations are dissolved in water, they will anyway thermodynamically be oxidized into Fe3+ cations by O2.72
(iv) Based on the GDE ICP-MS data at 20 °C that will be discussed later, the rate of production of dissolved Fe ions is assumed to be approximately two times faster in O2 than in Ar GDE experiments.
(v) A homogeneous potential distribution is assumed in the catalyst layer.
Considering the effect of increased Fe–N–C loading, the amount of 57Fe dissolution follows a linear trend over the initial 50 CVs (Fig. S6a, ESI†). The percentage of total 57Fe detected increases from 7.5 ± 2.9% to 15.2 ± 3.3% as catalyst loading increases from 0.05 to 0.40 mgFe–N–C cm−2geo, with 11.3 ± 5.6% at 0.20 mgFe–N–C cm−2geo (Fig. S6b, ESI†). This finding appears counterintuitive as one would expect either an equivalent percentage of Fe detected relative to the loading, or even a reduced percentage of detected Fe, due to reduced active site utilization with increasing thickness of the catalyst layer. It is also worth noting that there is a constant 130 ngFe gFeNC−1 s−1 57Fe concentration observed when held at 0.9 VRHE (Fig. 1a–c), which was also the OCP of the TAP 900@57Fe catalyst.
After the initial 50 CVs at 50 mV s−1, six CVs were conducted at 10 mV s−1 under Ar and then O2-saturation. With increasing TAP 900@57Fe loading under O2-saturation, the limiting current density (below 0.65 VRHE) only incrementally increases. This slight increase can be explained by the increasing thickness of the catalyst layer with loading, which penetrates deeper into the flowing O2-saturated electrolyte. Meanwhile, between 0.65–0.80 VRHE there is an increasing O2 reduction peak in the cathodic direction (Fig. S7a, ESI†). This is caused by a build-up of O2 concentration locally in the catalyst layer while scanning the potential region of 0.800–0.925 VRHE, where very little ORR is observed.
Under Ar-saturated conditions the current density increases proportional to the catalyst loading; we note there is an increasing peak on the cathodic scan (Fig. S7b, ESI†). We attribute this cathodic peak to the reduction of trace O2, arising from air ingress at the junction of the Kalrez O-ring and cell (or cavitation from the peristaltic pump). Still, the amount of O2 appears negligible. Normalizing the 57Fe detected to charge passed and catalyst loading shows the amount of 57Fe detected is constant under O2 but increases with reduced catalyst loading under Ar (Fig. S7c and d, ESI†). Meanwhile, the amount of 57Fe detected is equivalent under either gas saturation, with 1.3–2.0% of total 57Fe detected, and linear dependence with Fe–N–C loading (Fig. S7e and f, ESI†). Focusing on the dissolution at 0.2 mgFeNC cm−2geo, similar profiles are observed under Ar and O2-saturation (Fig. 1b).
To better distinguish the Fe dissolution features, slow CVs (1 mV s−1) were conducted under O2-saturation (Fig. 1c). The slow scans show two onsets of 57Fe dissolution above background levels on the cathodic scan at ca. 0.72 and 0.33 VRHE (Fig. 1c).
To evaluate differences in Fe detection and profiles over a longer period, 1 h AST or chronoamperometry (CA) were recorded in 0.1 M HClO4 (Fig. 2a and b) or 0.05 M H2SO4 (Fig. 2c). Greater 57Fe loading-normalized concentration is observed over the course of the AST under O2 than Ar. 57Fe concentration follows a slow decline under O2 and rapid plateau above baseline under Ar (Fig. 2a). 2.7 ± 0.1% of total 57Fe is detected during O2 AST (Fig. 2d), with a charge normalized Fe dissolution of 503 ± 3 ngFe mgFeNC−1 C−1 (Fig. 2e). Meanwhile, half 57Fe concentration is observed under Ar AST (Fig. 2d and Fig. S8, ESI†); however, normalizing to the total charge passed shows approximately double, with 1022 ngFe mgFeNC−1 C−1 (Fig. 2e). Pre- and post-mortem bright-field TEM of these samples shows no formation of detectable nanoparticles under Ar or O2 (Fig. S9, ESI†), indicating all Fe demetallation leads to dissolution at 25 °C, in agreement with former findings of Kumar et al.37
CA under O2 at 0.2 VRHE shows a large initial spike in 57Fe concentration, which then decays over time, while CA at 0.6 VRHE shows a smaller spike and lower overall dissolution (Fig. 2b). The initial spike in 57Fe concentration may be related to double layer charging and rapid change in potential. After 30 min, the current density and Fe dissolution are equivalent at 0.2 and 0.6 VRHE CA. CA at 0.2 VRHE ends with 4.6 ± 0.4% of total 57Fe and 686 ± 166 ngFe mgFeNC−1 C−1. This is approximately double the values at 0.6 VRHE, with 2.2 ± 0.1% 57Fe and 358 ± 61 ngFe mgFeNC−1 C−1 (Fig. 2e). This correlates with the observations from Fig. 1c, where greatest Fe dissolution occurs around 0.20 VRHE.
In 0.05 M H2SO4 instead of 0.1 M HClO4, O2 AST shows a similar dissolution profile, with lower Fe detection but higher O2 current densities (Fig. 2c). This difference in current is unexpected as O2 solubility is comparable at these acid concentrations. Meanwhile the total 57Fe loss is 2.3 ± 0.1% in 0.05 M H2SO4 and slightly higher in 0.1 M HClO4 with 2.7 ± 0.1% (Fig. 2d). However, the charge normalized Fe dissolution is less than half in 0.05 M H2SO4, at 231 ± 63 ngFe mgFeNC−1 C−1 (Fig. 2e). The presence of sulfate versus perchlorate will affect the Fe speciation and the mobility of Fe species.74 Additionally, the second acidity of H2SO4 is weak (Ka1 = 10+3, Ka2 = 1.26 × 10−2 = [H+][SO42−]/[HSO4−]) compared to HClO4, which completely dissociates (Ka = 10+9 = [H+][ClO4−]/[HClO4]).75 These results warrant future studies on Fe dissolution rates in HClO4 and H2SO4 with varying pH.
Based on flow cell results, 50 CVs under Ar-saturation (50 mV s−1, 0.9–0.2 VRHE, Fig. S10, ESI†) were initially carried out to remove loosely bound Fe. O2 reduction was measured in GDE half-cell before and after AST tests (Fig. 3a and b). Catalyst loadings varied between 0.7 to 1.0 mgFeNC cm−2geo, consequently corresponding mass activity plots are shown in Fig. S11a and b (ESI†). Compared to initial 20 °C O2 reduction, after 20 °C Ar AST there is an apparent improvement in O2 reduction performance at current densities up to −50 mA cm−2geo (Fig. 3a). This is assigned to improved wetting of TAP 900@Fe during the 20 °C Ar AST. Meanwhile, 20 °C O2 AST led to noticeable performance degradation after only 200 cycles, with potential shift at −50 mA cm−2geo of −50 ± 30 mV (from 0.61 ± 0.03 to 0.56 ± 0.00 VRHE,iR-free) compared to pristine 20 °C TAP 900@Fe (Fig. 3a). At −50 mA cm−2geo, 75 °C GDE pristine TAP 900@Fe shows an improved O2 reduction potential of 0.68 ± 0.01 VRHE,iR-free. Meanwhile, 75 °C O2 200 AST cycles results in severe degradation to 0.58 ± 0.03 VRHE,iR-free (Fig. 3b).
Within the pristine TAP 900@Fe GDE no visible nanoparticles >2 nm are detected using HAADF-STEM and STEM-EDXS spectrum imaging (Fig. 3d and Fig. S15a, ESI†); however, sub-nanometric Fe clusters below the detection limit of the microscope could be present, as observed in separate higher resolution HAADF-STEM measurements (Fig. S16, ESI†). After 20 °C Ar protocol, one large FexOy nanoparticle is detected in the spectrum image, while, at higher magnification, small clusters are observed (Fig. 3e and Fig. S15b, ESI†). Numerous Fe nanoparticles are observed following 20 °C O2 protocol in GDE, which are assigned to FexOy based on overlaying the Fe and O EDXS mapping (Fig. 3f and Fig. S15c, ESI†). HAADF-STEM combined with EDXS and EELS reveals clusters containing Ca and Fe in fresh and post Ar and O2 AST GDE (Fig. S16, ESI†). The presence of Ca remains unexplained, as we consistently used MilliQ water for all our electrochemical experiments and rinsing steps. No trace of Ca was also detected in the native catalyst. We therefore attribute it to contamination by tap water. The peak at 695 eV is from Fe–K. STEM-EELS analysis in regions without Fe particles cannot resolve any Fe peak (Fig. S16, ESI†), likely owing to the concentration of FeNx sites being below the limit of detection.
Post 75 °C O2 protocol no large FexOy particles are seen from EDXS and limited Fe clusters from HAADF-STEM (Fig. 3g and Fig. S15d, ESI†). No significant change from the pristine TAP 900@Fe structure is observed after 20 °C O2 and Ar protocols, (Fig. S17a–c, ESI†); however, after 75 °C O2 protocol a denser particle structure is observed (Fig. S17d, ESI†).
XRD on post-mortem GDE AST samples was conducted to try and deduce the type of FexOy, however either the lack of crystallinity, small particle size and/or low concentration meant no sharp peaks relating to Fe particles could be identified (Fig. S18, ESI†). The peak at 18.0° is assigned to polytetrafluoroethylene, which arises from the Nafion backbone. It is worth mentioning that pristine TAP 900@Fe does not show a graphite peak at ∼25.6° (002), suggesting its amorphous or graphene-like structure, with an average of single atomic layers found from previous Raman analysis.76
Normalized absorption and first derivative XANES of fresh TAP 900@Fe powder and GDE ink, plus post Ar and O2 25 °C protocols, are compared to references of Fe foil, FeO and Fe2O3 in Fig. S19a and d (ESI†). A positive shift of center of mass of the pre-edge in TAP 900@Fe ink and after Ar and O2 protocols signifies an increase of oxidation state, while their decrease in intensity is related to a change in local coordination of Fe. TAP 900@Fe GDE ink displays a near identical spectra to post 25 °C O2. This suggests changes in Fe coordination and oxidation state between TAP 900@Fe powder and its ink Post Ar protocol shows a lower rising edge position indicating a lower average Fe oxidation state, or change in bond length and/or coordination change.
For initial 20 °C Ar (Fig. 4a), Fe concentration above baseline occurs at 0.83 VRHE,iR-free and reaches a maximum concentration between 0.64–0.48 VRHE,iR-free. Returning to 0.83 VRHE,iR-free, Fe concentration returns to baseline levels. Initial 20 °C O2 current step holds (Fig. 4a) show a lower baseline Fe concentration than 20 °C Ar. A fall in Fe concentration below baseline levels is observed when increasing current density from −1 to −15 mA cm−2geo, corresponding to 0.85 ± 0.02 to 0.80 ± 0.01 VRHE,iR-free, respectively. When returning anodically to hold at −1 mA cm−2geo, Fe concentration increases and only begins falling back to baseline once returning to hold at −0.05 mA cm−2geo. Initial 75 °C O2 current hold measurements show a higher baseline Fe concentration, with increased Fe concentration during holds at −1 to −15 mA cm−2geo. Fe concentration then returns to approximate baseline values during holds at −50 and −100 mA cm−2geo, corresponding to 0.66 ± 0.04 and 0.62 ± 0.04 VRHE,iR-free, respectively. Returning anodically to holds at −15 and −0.6 mA cm−2geo results in increased Fe concentration.
Moving to online AST monitoring (Fig. 4b), 20 °C Ar shows increased Fe concentration at the beginning of the AST. Fe concentration then gradually decreases over time and falls back to baseline levels after the AST. To note, AST O2 have the same number of cycles (200) in protocol as Ar (3 s holds at each potential), but O2 ASTs took a longer duration because of the additional time to switch the applied current ranges between 3 s holds, which is not required in Ar AST protocol. During the AST, 20 °C O2 shows a similar Fe concentration profile to current hold prior to AST (Fig. 4a), with an initial Fe concentration spike, followed by reduced Fe concentration below baseline levels. Fe concentration then returns to baseline levels post AST, without displaying a dissolution spike. 75 °C O2 also shows an initial spike in Fe concentration at the beginning of the AST, but then maintains baseline Fe concentration values during and post AST with no discernable change.
Post AST (Fig. 4c), 20 °C Ar show Fe concentration significantly decreases across the whole potential range compared to prior to the AST (Fig. 4a). This suggests unstable Fe species have been depleted over the AST. Current step holds after 20 °C O2 AST show a similar Fe concentration profile to measurements prior to AST, although a higher Fe concentration spike is observed post AST when stepping from −1 to −15 mA cm−2geo (Fig. 4c). Post AST 75 °C O2 shows a symmetric Fe concentration profile when increasing and decreasing current. 75 °C O2 GDE ICP-MS results correlate with HAADF-STEM and STEM-EDXS observations (Fig. S15d, ESI†), where more Fe has dissolved rather than redeposited as particles, as is the case from 20 °C O2.
We note that the onset of increased 57Fe concentration at ca. 0.73 VRHE on the cathodic scan (Fig. 1c) coincides with the onset of the quinone–hydroquinone redox on the cathodic scan post 8000 O2 AST at 80 °C (Fig. 2c), and the second peak onset of increased 57Fe concentration at 0.33 VRHE on the cathodic scan coincides with the onset of the second reversible redox on the cathodic scan. Our observations suggest that the stability of the Fe centre may be intrinsically linked to the chemistry of the surrounding ligands; this notion is analogous to relationships observed by others between the catalytic activity and the chemistry of the surrounding ligands.24,77
We also note an initial exponential decay in Fe concentration (Fig. 1a), which was also observed by Choi et al. for their Fe–N–C catalyst.19,27 In our case maximum Fe concentration is observed instantaneously upon potential cycling in Ar, whereas in the report of Choi et al. maximum Fe concentration is reached after 2–3 CVs.19,27 This could be due to the vastly different catalyst structures between our highly micro- and mesoporous TAP 900@57Fe with high active site utilization,44 and the bulky particle and predominantly microporous ZIF-8 derived Fe–N–C of Choi et al.19,27 Alternatively, it could arise from mass transport effects from slow residence time in Choi et al.'s flow cell design. The structure of unmodified microporous ZIF-8 derived materials would have impeded mass transport, low active site utilization and therefore delayed detection of Fe dissolution. Differences in experimental setup and residence time calibration in this work and that of Choi et al. could also contribute to the observed time difference in Fe concentration detection.
Choi et al.27 detected ∼3% of total Fe over their initial 20 CVs in Ar-saturation (100 mV s−1, 0.8 mgFe–N–C cm−2) for their purely microporous ZIF-derived wet synthesis Fe–N–C containing FexC and Fe particles. Meanwhile their dry synthesis or post chemical or electrochemical modification significantly reduced the initial Fe dissolution.27 On the other hand, after 50 CVs (50 mV s−1, 0.4 mgFe–N–C cm−2), TAP 900@57Fe shows 15.2 ± 3.3% Fe detected. This again points to the different porosity and structure in TAP- and ZIF-derived materials, leading to different accessibility of Fe sites. It also appears that while our decoupled wet-synthesis approach for TAP 900@Fe avoided the formation of Fe particles,44 it still leads to significant Fe dissolution during initial CVs. Additionally, it should be noted, according to our previous ex situ TAP900@57Fe Mössbauer assignments, ca. 11% of the Fe existed as inactive FeCl2·4H2O.44 This species may represent some or all of the initially dissolved Fe species.
In Fig. 2a, the rapid decay and plateau in Ar-saturation may be explained by the sudden step in potential, causing dissolution of inactive Fe species, with varying residence time of Fe across the catalyst layer. Meanwhile in O2-saturation the gradual decrease in Fe concentration is assigned from the decreasing concentration of highly active but unstable Fe species which dissolve during the O2 reduction cycle. Such unstable and dissolving FeNx sites have been previously assigned to high spin Fe3+Nx sites from 57Fe Mössbauer spectroscopy,38 which were previously found to make up the most significant portion of Fe species in TAP 900@57Fe.44
Results from Fig. 1b (Fig. S7e and f, ESI†) suggest that the Fe concentration is independent of O2 reduction under cyclic voltammetry (0.9–0.2 VRHE at 10 mV s−1) in flow cell. This is contrary to what is observed in Fig. 2a, where detected Fe concentration is greater under O2 than Ar under AST (step from 0.9 to 0.6 VRHE with 3 s potential holds) flow cell conditions. These different Fe concentrations may be due to either the different potentials scanned (AST: 0.9–0.6 VRHEversus CV: 0.925–0.2 VRHE), the potential scanning protocol (AST: 3 s square wave voltammetry holds versus CV: 10 mV s−1), or 6 CVs not providing enough cycles to distinguish changes in Fe concentration. Unfortunately, the ICP-MS drift during flow cell operation prevented running a greater number of CVs to test this hypothesis.
Considering Fig. 2e and Fig. S8 (ESI†), Zelenay and coworkers also observed from ex situ ICP-MS that HClO4 dissolved more Fe from their polyaniline-derived Fe–N–C than H2SO4, which they attributed to differences in solubility of Fe perchlorates and sulfates.31 We suggest this observation could also be attributed to the stronger SO42− binding on the Fe site,78 whereas ClO4− has been proposed to mimic non-specifically adsorbing properties of perfluoro sulfonic acid ionomers.79 If true, this would imply AST measurements in H2SO4 in RDE and GDE would lead to slower Fe–N–C degradation than in HClO4 (at the same pH), when Fe dissolution is the main degradation mechanism.
The different current density under 0.1 M HClO4 and 0.05 M H2SO4 (Fig. 2a and c) may be related to kinetic effects of the proton donor.80 Additionally, at 0.8 VRHE Fe–N–Cs have recently been reported to possess 1.3–2.9 higher mass activity in H2SO4 than HClO4.78
The rapid decay in O2 reduction performance (e.g. −50 ± 30 mV at 50 mA cm−2geo after 200 cycle AST in 20 °C O2) and high Fe dissolution can be attributed to the high percentage of unstable high spin Fe3+Nx present (assuming the same type of sites are present between TAP 900@57Fe and TAP 900@Fe). Additionally, according to density functional theory (DFT) calculations for Fe–N–C, the number and size of graphene sheets affects the Fe dissolution potential.81 Previous Raman analysis of TAP 900 determined an atomically thin carbon structure,76 which therefore leads itself to possess less stable FeNx sites.
The online GDE ICP-MS concentration profile under 20 °C O2 (Fig. 4a and c) suggests Fe dissolution and subsequent detection by ICP-MS at low current density (−0.05 to −1.00 mA cm−2geo). Meanwhile, at higher current density (−15, −50 and −100 mA cm−2geo), a process of Fe dissolution and redeposition locally into FexOy in the catalyst layer is proposed. This is supported by the increased observation of FexOy after O2 GDE protocol from HAADF-STEM and EDXS (Fig. 3f and Fig. S15, ESI†). The reason for FexOy formation is hypothesized to arise based on the Fe Pourbaix diagram, where an increase in the local pH would form Fe2O3. This pH increase in the catalyst layer could occur due to the rapid consumption of H+ during increased O2 reduction currents (4H+ + O2 + 4e− → 2H2O). It is then expected that some FexOy redissolves when returning anodically to low O2 reduction current density (−1 mA cm−2geo), due to a return to acidic pH. This redissolution is evidenced by the detected increase in Fe concentration at −1 mA cm−2geo on the anodic step for 20 °C O2 in GDE ICP-MS. The observation of FexOy corroborates previous findings from post-mortem O2 AST protocols.37,38 Moreover, the increased Fe concentration detected when stepping the potential down in the cathodic direction after post AST (Fig. 4c) for O2 GDE at 20 °C and 75 °C supports the hypothesis that FexOy builds up in the catalyst layer at current densities of −50 mA cm−2geo during the AST and is only released at lower current density holds (−1 mA cm−2geo at 20 °C and 75 °C).
We previously reported the extensive characterisation of as-prepared TAP 900@Fe, confirming the purely atomic dispersion as a pristine powder (XAS, cryo 57Fe Mössbauer and HAADF-STEM).44 A clear average change in oxidation and coordination is observed from TAP 900@Fe powder to electrode. Therefore, it appears sub-nanometric/small Fe clusters (<2 nm) form during electrode preparation (Fig. 3 and Fig. S15, S16, ESI†). This matches the recent report of Saveleva et al. who found, based on XAS, the ink preparation of the electrode can lead to significant changes in Fe in Fe–N–Cs from the catalyst powder to the electrode.43
We note that the similar XANES signals of TAP 900@Fe ink (Fig. S19, ESI†) and post O2 protocol are contrary to observations from HAADF-STEM (Fig. 3). This can be explained by the different probing regions of the techniques, with XANES examining the bulk electrode, where local deviations of low concentration large particles can remain hidden, which can be resolved by HAADF-STEM.
Meanwhile, the negative shift of the lower rising edge position in XANES from post 20 °C Ar protocol (Fig. S19, ESI†) is likely due to significant dissolution of Fe species with higher oxidation state, or a change in average bond length and/or coordination change.
Mass transport (O2 solubility and H+) and the thermodynamics and kinetics of ORR and Fe dissolution (at a constant potential on the RHE scale) will all change with temperature.84 This makes it challenging to deconvolute their contributions to changes in performance; however, kinetic modelling based on experimental data can help explain phenomena, such as local pH changes.
Fig. 5 (a) Schematic depicting kinetically modelled system. (b) Initial GDE-ICP-MS data in terms of [Fe]. Simulated Fe concentration over (c) Time and (d) Catalyst layer. (e) pH and subsequent potential vs. RHE distribution across catalyst layer (assuming Nernstian potential shift with pH). kr is the proton consumption rate constant and ε is the void volume. (f) Pourbaix diagram of Fe surface at 25 °C and [Fe] = 10−6 M with labelled points under O2 (−15 mA cm−2geo) and Ar (0 mA cm−2geo) conditions. The error bar for O2 represents variation of pH from different ε and kr in Fig. 5e. Fe Pourbaix diagram replotted from ref. 87. |
Fig. 5e displays the corresponding simulated pH profile in the catalyst layer. The simulations predict a significantly lower concentration of detected Fe cations during O2 reduction (Fig. 5d). This phenomenon is attributed to the precipitation of Fe3+ cations under the local conditions in the catalyst layer, with the Fe concentration resulting from the balance between Fe precipitation and redissolution. Indeed, simulations indicate that at −15 mA cm−2geo, the local pH at the interface between the Fe–N–C layer and the electrolyte solution is approximately 1.5 (Fig. 5e). There is then a substantial and rapid increase in pH moving into the bulk catalyst layer (far from the liquid electrolyte), reaching pH values ca. 8–9. We note that the effect of Ca contamination (Fig. S16, ESI†) would be minor since we do not have evidence of local pH change under Ar and highlight that the presence of Ca2+ would be expected to decrease the pH rather than increase the pH (Ks = 6.46 × 10−6).88
In terms of potential, the pH increasing to 8–9 is equivalent to ca. 1.1 V (Fig. 5e), based on Nernstian shift. Consequently, only the region of the catalyst layer near the solution contributes to O2 reduction, implying Fe–N–C thickness should be minimised, as previously proposed by Litster and coworkers from PEMFC modelling for maximised power (<30 μm).11 We therefore propose under practical operating current it is not possible to synchronize the pH across the catalyst layer, due to proton consumption. This supports the results of Banham et al. who found improved stability based on lower equivalent weight ionomer, which have increased ionic conductance.41 We also note from their qualitative reaction zone scheme that Fe–N–C degradation would not be as severe under air due to reduced O2 concentrations41 and therefore reduced proton consumption.
Aside from minimising Fe–N–C electrode thickness, catalyst structure modifications can be made, based on bio-inspiration.89 For instance, the enzyme-inspired architecture proposed by Xia et al.90 where protons and electrons are transported to the active site via ordered proton-conducting and electron-transporting channels. This is similar to the proposal of Middelman,91 who suggested the controlled self-assembly of electrodes. Methods can be adapted from the battery community who use thick electrodes (>100 μm),92 such as ice templating and graded electrodes.
Considering high loading Fe–N–C (thick) cathodes, one can envisage that the rate of degradation observed decreasing, as more Fe–N–C is available to react as the reaction zone passes across the degrading catalyst layer (from the membrane to backside of the Fe–N–C). Meanwhile, the intrinsic stability number93 of the FeNx sites (ratio between the number of moles of Fe ions dissolved and the number of moles of oxygen being reacted) should remain the same, all else being equal.
The conditions on the Fe Pourbaix diagram are depicted in Fig. 5f. For the parameter values considered, >90% of the Fe–N–C layer experiences pH > 2.4, which would result in formation of Fe2O3 at ∼0.7 VSHE, for an Fe surface. Pourbaix diagrams are dependent on temperature and concentration of species. While it appears [Fe] is in order of 10−6 M, the Pourbaix diagram for [Fe] = 10−8 M at 25 °C can be found for comparison in Fig. S21 (ESI†). Additionally, Pourbaix diagrams were developed from metal surfaces rather than single atoms, where DFT-based models have instead been developed,81 although here it is appears the Fe–N–C system is sufficiently represented by the Pourbaix diagram of an Fe surface.87
1. The fate of Fe (and other metal species) can vary through-plane of the catalyst layer. Therefore, the heterogeneity of Fe–N–C degradation should be considered when conducting operando and post-mortem studies.
2. Precious metal-free layers in PEMFCs, which typically employ 60–100 μmM-N-C thick cathodes,7 may not utilize the majority of the catalyst layer during O2 reduction due to proton consumption. Focus, therefore, should be made on decreasing the electrode thickness by further increasing the electrochemically accessible volumetric active site density of precious metal-free catalysts. This could be facilitated by ink and ionomer optimisation (higher conductance, less bulky ionomer and tuning the ionomer:catalyst ratio), as well as designing more accessible and ordered catalyst pore structures.
Footnotes |
† Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d4ee01995d |
‡ These authors contributed equally. |
This journal is © The Royal Society of Chemistry 2024 |