Kenza Elbouazzaoui,
Charles Aram Hall
,
Kristina Edström
,
Jonas Mindemark
and
Daniel Brandell
*
Department of Chemistry – Ångström Laboratory, Uppsala University, Box 538, SE-751 21, Uppsala, Sweden. E-mail: Daniel.Brandell@kemi.uu.se
First published on 25th July 2025
While polymer-based solid-state sodium batteries promise both safe operation and utilization of sustainable materials, they are held back by the insufficient ionic conductivity of the involved solid polymer electrolytes (SPEs). In this study, the conductivity and cation transference number are significantly improved through the construction of a composite polymer electrolyte (CPE) system based on poly(trimethylene carbonate) (PTMC) with sodium bis(trifluorosulfonylimide) (NaTFSI), combined with NaAlO2 (NAO) ceramic filler at loadings ranging from 10 to 40 wt%. The NAO-based CPEs show the highest conductivity at 20 wt% NAO, with a Na+ transference number of ∼0.9 at 60 °C also being obtained for the same material, which is notably higher than that for the NAO-free SPE. Solid-state batteries composed of a Prussian white cathode and a Na metal anode and employing these CPEs reach a cycling performance of ∼100–150 mA h g−1 at C/10 and 55 °C for more than 200 cycles without additives or plasticizers, thus opening the door to the potential exploration of CPEs for Na-based battery chemistries.
Both solid polymer electrolytes (SPEs) and solid inorganic electrolytes (SIEs) have been explored for Na-based SSBs.5 Sodium β- and β’’-Al2O3,6,7 NASICON structures (e.g. Na3Zr2Si2PO12; “NZSP”),8,9 and sulfides (e.g. Na3PS4 and Na3SbS4)10,11 constitute state-of-the-art Na-based SIEs, many of which can exhibit good ionic conductivity at room temperature (>10−4 S cm−1) and a high Na+ transference number (T+ ∼1). However, implementing SIEs in solid-state Na batteries is technically challenging and results in high interfacial resistances due to the rigid solid/solid interfacial contacts.12 This is a common disadvantage related to SIE-based batteries, almost regardless of the cell chemistry. SPEs can, on the other hand, present an efficient strategy to address this problem thanks to their flexibility and soft nature, enabling better interfacial contact with the electrodes. However, SPEs typically display shortcomings related to low ionic conductivity and transference number, limiting their applications in Na-based SSBs.
Equivalent to Li-based SPEs, poly(ethylene oxide) (PEO) has also shown potential in Na-based SPEs. Qi et al., for example, fabricated a SPE made of PEO combined with sodium bis(fluorosulfonyl)imide (NaFSI) salt, which showed a moderate ionic conductivity of 4.1 × 10−4 S cm−1 and a Na+ transference number of 0.16 at 80 °C.13 This combination of comparatively high SPE conductivity but poor cationic transference is typical of PEO-based SPEs. In contrast, polycarbonates have also been explored as SPEs for Na-based systems.14 Sångeland et al. reported an SPE made of poly(trimethylene carbonate) (PTMC) with NaFSI salt, and showed that the ionic conductivity can reach >10−4 S cm−1, with a moderate T+ of 0.48 at 80 °C for the highest NaFSI concentration investigated.15 A similar behavior was recently reported for polypropylene carbonate (PPC) with NaFSI, showing that an increase in ionic conductivity can be achieved with high NaFSI salt content, reaching ∼1 mS cm−1 at 80 °C at the highest investigated salt concentration of ∼84 wt%.16
Even though these highly concentrated SPE materials can display promising conductivity values, applications of SPEs in Na-based SSBs are likely more difficult to achieve due to limited mechanical properties. Moderate salt concentration will likely be necessary to achieve long-term battery operation, but these materials generally display limited conductivities. Alternative strategies to raise conductivity and transference numbers are therefore necessary. One such strategy is through combining a polymer and a ceramic material into a so-called composite polymer electrolyte (CPE). While extensive efforts have been dedicated to the development of CPEs for Li-based systems, the research into Na-based counterparts is much more limited.17 In particular, CPE development has focused on the use of NASICON-type active (i.e., ion-conductive) ceramic fillers such as Na3Zr2Si2PO12,18 Na3.4Zr1.8Mg0.2Si2PO12,19 Na3.4Zr1.8Mg0.2Si2PO12,20 and Na3.4Zr1.9Zn0.1Si2.2P0.8O12 in PEO-based SPEs.21 It is noteworthy that while these reported Na-based CPEs exhibit better ionic transport and improved battery properties as compared to the pristine PEO-based SPEs, their performance is in many cases also largely dependent on the contribution arising from additives other than the ceramic fillers, such as liquid electrolytes or plasticizers.17 Furthermore, many of these positive effects reported can be attributed to the decreased crystallinity of PEO or interfacial effects rather than to ion transport contributions from the actively conductive materials themselves. Passive (non-conductive) ceramic fillers should thereby be able to generate similar improvements in performance, but have not yet received equal attention. Using simple ceramic fillers such as SiO2 and ZrO2,22–25 some success has been seen; e.g., Scrosati et al. reported a CPE based on a PEO:
NaTFSI matrix with 5 wt% SiO2, delivering an ionic conductivity reaching ∼1 mS cm−1 at 80 °C and a T+ of 0.51 at 75 °C.26 While this clearly indicates the potential impact of implementing CPEs for Na systems based on low-cost and sustainable passive fillers, it also highlights the need for a better understanding of the functionality of the fillers in CPEs and their role and usefulness for Na-SSB development.
We have in recent work studied Li-based CPEs with the passive filler γ-LiAlO2 incorporated into PTMC.27 The material showed a large boost in conductivity as compared to the filler-free counterpart, a very high cationic transference number close to unity and also promising Li-battery performance. In this work, we study an analogous PTMC-based CPE platform with γ-NaAlO2 ceramic filler as a direct Na-based counterpart. This constitutes the first exploration of non-polyether CPEs for Na-based SSBs. PTMC is chosen due to its amorphous nature, making it possible to directly observe the effect of ceramic fillers on the ionic conductivity without the results being obscured by changes in the degree of polymer crystallinity. Similar to the γ-LiAlO2 CPE system, the addition of 20 wt% γ-NaAlO2 is shown to give a clear performance boost to the ionic conductivity and Na+ transference number. Finally, the material is evaluated through galvanostatic charge–discharge cycling in battery cells comprising a Prussian white cathode and a Na-metal anode.
Cationic transference numbers were investigated electrochemically employing the Bruce–Vincent method30 on a BioLogic SP-240 potentiostat at 60 °C. Before and after applying a potentiostatic polarization of 10 mV, the cell impedance was measured from 7 MHz to 100 mHz. Symmetrical pouch cells for the measurements were assembled using SPE/CPE films of 16 mm diameter sandwiched between two 13 mm sodium disks. The cells were kept at 60 °C overnight prior to measurements. The sodium transference number T+ was determined from eqn (1):
![]() | (1) |
Prussian white (NaxFe[Fe(CN)6]) powder from Altris was used as received as the cathode active material. A full characterization of this material can be found in ref. 31. Positive electrodes were prepared by mixing Prussian white in a water-based slurry with a carboxymethyl cellulose (CMC) binder and conductive carbon additive (Enasco 250P). The slurry composition was 85:
10
:
5 (w/w) for Prussian white, carboxymethyl cellulose and conductive additive. Slurries were cast on carbon-coated aluminum foil at 100 μm thickness (wet coating), resulting in an areal mass loading of ∼1 mg cm−2. These were punched to 13 mm diameter electrodes.
Electrochemical characterization was performed using a pouch cell configuration with metallic sodium as the negative electrode. Prior to assembly, the Prussian white electrodes were dried under vacuum at 170 °C for 15 h inside an Ar-filled glovebox (O2 and H2O < 0.5 ppm). Sodium electrodes were prepared in a glovebox from sodium cubes by pressing cleaned Na onto aluminum foil using a hydraulic press. Current collectors in the pouch cells were made of Al foil. Pouch cells were assembled with the CPE (16 mm in diameter) sandwiched between a cathode of 13 mm diameter and a sodium disk of 15 mm diameter. Galvanostatic cycling tests were carried out with an ARBIN BT-2043 on the lab-scale pouch cells. Cycling was performed at C-rates calculated based on a practical capacity of ∼150 mA h g−1 for the Prussian white material. Practically, cycling was carried out initially from a C-rate of C/10 up to 5C within a voltage window of 2.0–4.0 V at room temperature and 55 °C.
As displayed in Table 1, both Na and Li aluminates share the same P41212 space group and have similar unit cell parameters, indicating that NAO crystallizes in the same way as LAO with a tetragonal symmetry.
γ-NaAlO2 | |
---|---|
Space group | P41212 (92) |
Unit cell parameters | a = b = 5.16558 ± 0.00009 Å |
c = 6.2811 ± 0.0001 Å | |
α = β = γ = 90° | |
Unit cell volume | V = 167.599 ± 0.007 Å3 |
The filler-free PTMC:
NaTFSI SPE and PTMC
:
NaTFSI
:
NAO CPEs were prepared by a solution casting method, which has been used previously to fabricate CPEs with LiTFSI and LiAlO2.27 As described in the experimental section, an additional step of ball-mill mixing is needed to ensure homogeneity of the solution containing PTMC, NaTFSI and NAO particles. Therefore, it is essential to verify that all CPE components are structurally stable, and that the addition of NAO particles does not change the characteristics of the polymer matrix. As shown in Fig. 2a, all characteristic peaks of NAO particles are maintained for all CPEs from 10 up to 40 wt%, indicating that the γ-phase is indeed stable and does not undergo any structural changes. Since PTMC is a fully amorphous polymer, no effect of reduced polymer crystallinity is expected after incorporating NAO particles. The chemical fingerprint of the polymer matrix was examined by FTIR spectroscopy. Fig. 2b depicts the FTIR spectra of electrolytes with and without NAO particles, also including peak assignments of the C
O stretch vibration. Since PTMC is a polycarbonate, it shows the characteristic C
O stretch at approximately 1740 cm−1, which shifts towards lower wavenumbers when it coordinates to cations, i.e., in this case sodium ions.39 This behavior is also observed for the system composed of PTMC with NaTFSI salt, and is unchanged after incorporating the NAO ceramic filler regardless of loading. Additional peaks in the fingerprint region are much more difficult to clearly assign and this region is largely unaffected by the addition of the NAO particles.
![]() | ||
Fig. 2 (a) XRD patterns of the as-synthesized NAO particles and PTMC-based CPEs; (b) FTIR spectra of the filler-free SPE and CPEs (NAO loadings from 10 to 40 wt%). |
The fabricated SPE and CPEs were assembled in coin cells with blocking stainless steel electrodes to evaluate the influence of adding NAO ceramic filler on the ion conduction properties of the PTMC:
NaTFSI electrolytes. The temperature dependence of the ionic conductivity is displayed in Fig. 3a, and exhibits the typical Vogel–Fulcher–Tammann (VFT) type of behavior expected of amorphous polymers where the ionic transport is coupled to polymer segmental motion. The ionic conductivity of the filler-free SPE is in good agreement with data previously reported for the same PTMC
:
NaTFSI system at approximately the same NaTFSI salt concentration.40 Upon incorporating 10 or 20 wt% of NAO particles, the conductivity significantly increases to higher values within the entire investigated temperature range, but without any changes in the shape of the curves. This indicates that similar ion transport mechanisms are effective in all samples, even after addition of NAO particles, and is consistent with the formation of uniform films with dispersed particles (see Fig. S4†). Above 20 wt% ceramic filler loading, the ionic conductivity decreases. This behavior was also observed for PTMC
:
LiTFSI
:
LAO CPEs, and has been attributed to particle agglomeration; leading to less polymer–ceramic interface area, tortuosity effects and dilution of the conductive SPE phase.27 Nevertheless, it is interesting that the ionic conductivity above 20 wt% NAO still remains higher than the conductivity of the filler-free reference SPE. In comparison with other solid-state Na-conductors, however, the total ionic conductivity is not exceptionally high (see Table S1†); this reflects the use of PTMC as the polymer host.
The increase in the ionic conductivity by one order of magnitude should be considered significant. This also reflects a similarity between the LAO and NAO ceramic fillers for Li- and Na-based systems, respectively. Therefore, it is likely that the reasons behind the improved ionic conductivity for NAO-based CPEs are similar to those for LAO-based CPEs; i.e., an accumulation of anions at the particle surfaces creates additional ion transport pathways along the polymer–ceramic interfaces, combined with improved ion–ion separation.
Based on the ionic conductivity data, the CPE with 20 wt% NAO particles (denoted as CPE20NAO) exhibits the highest ionic conductivity across much of the explored temperature range, and was therefore chosen for measurement of the Na+ transference number. While the Bruce–Vincent method is relatively easy to apply to Li systems, the experiment is much more challenging for Na systems because of the difficulty in reaching a stable steady-state current after polarization due to instability at the interface between the electrolyte and sodium metal.41 While it was indeed difficult to properly determine the T+ from the filler-free SPE due to such instabilities, the CPE20NAO successfully enables sufficient interfacial stability against Na metal. As displayed in Fig. 4, a steady-state current was reached after 80 min of potentiostatic polarization, and using eqn (1), a Na+ transference number of 0.92 at 60 °C was determined for the CPE containing 20 wt% NAO particles. This value far exceeds the T+ reported for the PTMC:
LiTFSI SPE (∼0.8 at 60 °C),42 and is also higher than that for a PTMC-based SPE with NaFSI (∼0.48 at 80 °C).15 This is by far the highest transference number reported for a PTMC-based Na-conducting electrolyte, and is consistent with the T+ obtained for the PTMC
:
LiTFSI-based CPE with LAO particles.27
![]() | ||
Fig. 4 (a) Chronoamperogram of CPE20 in a Na-metal symmetrical cell; (b) Nyquist plot of the same cell obtained before and after polarization. The interfacial resistance is determined after fitting using an appropriate equivalent circuit.28 The experiment was carried out at 60 °C. |
The clear improvement in Na+ conduction in the NAO-containing CPEs should also be beneficial for use in Na-metal battery cells. To this end, the CPE with 20 wt% NAO particles was employed in solid-state Na-metal batteries, composed of a Prussian white cathode, a Na metal anode, and the CPE20NAO electrolyte. When gentle pressure was applied over the pouch cell, CPE20NAO demonstrated promising electrochemical performance in fully solid-state Na-metal batteries at a C-rate of C/10 and at an operating temperature of 55 °C, as can be seen in Fig. 5. An initial capacity of 145 mA h g−1 was recorded while the initial coulombic efficiency was above 99%. A few scattered datapoints are observed during cycling, which can be explained by a possible occurrence of side reactions due to sodium salt decomposition.43 However, the incorporation of NAO particles is most likely contributing to the inhibition of side reactions through stabilization of the sodium salt through a similar effect as previously observed for the LAO-based CPEs.27 After 200 cycles, 54% of the initial capacity was retained with a coulombic efficiency of ca. 99%.
To improve capacity, rate-performance and room temperature performance, a wetting approach with liquid electrolytes was employed to ensure better interfacial contacts between the electrodes and electrolyte than in a full solid-state configuration. Thereby, a battery cell in the pouch cell configuration was assembled, composed of a Prussian white cathode, a Na metal anode, and the CPE20NAO electrolyte to which 40 μL of 1 M NaFSI in EC:
DEC (vol 1
:
1) was added. Galvanostatic cycling was carried out at an initial C-rate of C/10 and at room temperature, and an initial capacity of ∼143 mA h g−1 and a coulombic efficiency of 97.5% were recorded. The Na-metal battery cell displayed stable cycling, as seen in Fig. 6a, indicating the formation of stable electrolyte/electrode interphases that help circumvent the occurrence of side reactions. In previously reported studies on PTMC-based SPEs with a Na salt, erratic cell behavior was observed due to salt decomposition and associated to parasitic reactions.15 The results here thus further suggest that there is a positive effect on the electrochemical stability of the PTMC-based SPE when NAO particles are incorporated. Furthermore, the rate performance of CPE20NAO in Na-metal batteries was evaluated by cycling the battery while increasing the C-rate up to 5C. As shown in Fig. 6b, the cell capacity gradually decreases with the increasing C-rate; however, the battery cell shows a fairly high capacity at all rates, being higher than ∼92 mA h g−1 even at 5C.
It is important to note that the possibility of cycling such a battery cell at room temperature and at high C-rates depends on the addition of liquid electrolyte, which also plasticizes the SPE and reduces the resistivity of the CPE. However, these additives can be consumed by interfacial reactions with the electrode materials during long-term operation, causing battery failure or instabilities. Therefore, the interfacial electrode/electrolyte should be improved by means of a different strategy other than liquid electrolyte wetting, and further solid-state cell engineering techniques are necessary, e.g. the use of oligomeric coatings and tailoring of the electrode composition, porosity and the applied pressure. Nevertheless, the results indicate that it is not primarily the bulk conductivity of the solid-state CPE materials which is the main hurdle for successful battery operation, but rather the interfacial properties between the electrode and electrolyte – most likely on the cathode side – which are facilitated by the addition of small amounts of liquid. That the plateaus in the galvanostatic cycling data are clearly visible and located at the same voltages in Fig. 5a and 6a indicates the functionality of the solid-state electrolyte. These results thereby open the door towards further optimization of the battery design and composition to realize CPEs for solid-state Na-metal batteries.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d5ta03403e |
This journal is © The Royal Society of Chemistry 2025 |