Shenggong
He‡
a,
Shaofeng
Wang‡
a,
Hedong
Chen‡
a,
Xianhua
Hou
*a and
Zongping
Shao
*bc
aGuangdong Provincial Key Laboratory of Quantum Engineering and Quantum Materials, Guangdong Engineering Technology Research Center of Efficient Green Energy and Environment Protection Materials, Engineering Research Center of MTEES (Ministry of Education), School of Physics and Telecommunication Engineering, South China Normal University, Guangzhou 510006, China. E-mail: houxianhua@m.scnu.edu.cn
bJiangsu National Synergetic Innovation Center for Advanced Materials (SICAM), State Key Laboratory of Materials-Oriented Chemical Engineering, College of Chemical Engineering, Nanjing Tech University, Nanjing, 210009, China. E-mail: Shaozp@njtech.edu.cn
cWA School of Mines: Minerals, Energy and Chemical Engineering (WASM-MECE), Curtin University, Perth, WA, 6845 Australia
First published on 3rd January 2020
Supercapacitors that store energy through dual electrochemical layer capacitance or surface faradaic redox reactions are characterized by their fast charging/discharging capability, high power densities, and long cycling lifetime. However, the low energy density of supercapacitors seriously inhibits their practical applications. Herein, a dual-ion hybrid energy storage system using expanded graphite (EG) as the anion-intercalation supercapacitor-type cathode and graphite@nano-silicon@carbon (Si/C) as the cation intercalation battery-type anode is designed for efficient energy storage. The Si/C anode, synthesized by interfacial adhesion between nanosilicon and graphite with the help of pitch, demonstrates high specific capacity, remarkable cycling stability, and enhanced rate capability. Meanwhile, the EG cathode, which stores energy based on electrochemical double layer capacitance through its unique faradaic pseudocapacitive negative anion intercalation behaviour, demonstrates high energy densities of 462.9–356.5 W h kg−1 at power densities of 403–7130 W kg−1. The resulting Si/C//EG hybrid system delivered highly attractive energy densities of 252–222.6 W h kg−1 at power densities of 215–5420 W kg−1, which are superior to those of conventional electrochemical double layer capacitors and lithium-ion capacitors, making the dual-ion hybrid system a new type of energy storage device capable of achieving fast and efficient energy storage.
Considering the limited theoretical capacity of the LiCoO2 cathode and graphite anode, ternary LiNi1−x−yCoxMnyO2 cathodes (LNCM, with a theoretical capacity of 280 mA h g−1) and Si-based anodes (Li15Si4, 3580 mA h g−1) have been extensively exploited in recent years.10–12 By applying the ternary LNCM cathode, the energy density of LIBs can reach a theoretical value of 241 W h kg−1.13 However, big concerns about the ternary lithium batteries are their poor electrochemical stability at high voltage and poor rate performance. Due to the similar cation size of Li+ and Ni2+, the dislocation of the Li+ and Ni2+ may easily occur, resulting in reduced cycling stability and reversible capacity. In addition, ternary cathode materials usually show poor thermal stability, and may easily react with liquid electrolyte at high temperature leading to dramatic performance degradation. In addition, the poor lithium-ion conductivity of LNCM, which introduces large polarization resistance at high rates, accounts for poor rate performance.14–17
Supercapacitors, another type of extensively investigated electrochemical energy storage device distinguished by high power density and cycling stability, store energy through electrochemical double layer capacitance at the surface of both electrodes.18–20 However, such supercapacitors usually show relatively low energy density inferior to that of conventional LIBs.21–23 By introducing pseudocapacitance into the electrodes, the energy storage performance is enhanced through surface faradaic redox reactions, and consequently the capacity can be greatly improved. Up to now, the highest energy density of supercapacitors based on pseudocapacitance has been reported to be around 100 W h kg−1,24 which is however still inferior to that of conventional LIBs. Recently, supercapacitors based on a battery-like ion-intercalation mechanism have received considerable attention showing the capability of increasing energy density.25–28 Both cation-intercalation and anion-intercalation have been reported for supercapacitors. Up to now, an energy density as high as 231.7 W h kg−1 has been reported,29 which is already comparable to that of conventional LIBs with the LiCoO2 cathode and graphite anode. In order to reach further improvement of energy density, new advances in the materials composition and energy storage mechanism should be exploited.
Considering the high energy density of LIBs and high power density of supercapacitors, a new type of electrochemical system called the hybrid energy storage system was proposed. In this system, one electrode (typically the cathode) stores charge by a supercapacitor behavior, while the other electrode stores energy via conventional LIB behavior, so that it could have the advantages of both the supercapacitor (high power density and cycling stability) and the battery (high energy density).30–34 It is highly promising as the next-generation electrochemical storage device. Note that, due to the capacity limit of the supercapacitance electrode, the energy density of the reported devices is yet still lower than that of the conventional LIBs.29
For the above-mentioned energy storage devices, LIBs, supercapacitors and the hybrid system, the lithium ion plays roles in adsorption or intercalation. More recently, dual ion batteries, in which both the cation (lithium ion) and anion (PF6−) can be used for energy storage, have received considerable attention.35–38 The theoretical energy density can be further improved. However, the lack of suitable electrodes limits the energy density of dual ion batteries to be lower than 200 W h kg−1.39,40 Taking advantage of the dual-ion battery system, a special dual-ion hybrid electrochemical device constructed using a high voltage supercapacitor-type cathode and a battery-type anode via a dual-ion mechanism may lead to the achievement of high energy density, power density and cycling stability. Although many attempts have been made, the reported energy density is still lower than that of conventional LIBs.41
Here we report a new dual-ion hybrid electrochemical system that optimizes the supercapacitor-type cathode and battery-type anode to boost energy density, achieving an ultrahigh energy density of up to 252 W kg−1 (under a power density of 215 W kg−1), which is much superior to those of most of the available supercapacitors and dual-ion batteries, and even comparable to those of LIBs. In addition, the rate performance is obviously improved. The system maintains an energy density of 222.6 W h kg−1 even at a high power density of 5420 W kg−1. Also, the hybrid electrochemical energy storage system demonstrates superior cycling stability with a capacity retention of 94.6% after 1000 cycles at a 1C rate. The outstanding performance is reached by taking the use of an expanded graphite as an anion-intercalation-type pseudocapacitor cathode and a battery-type Si–graphite anode for energy storage.
The galvanostatic charging and discharging tests used a Neware BTS-3S test system. The hybrid cell full device was cycled within a voltage window of 3.0 and 5.0 V, and the rate capability was evaluated using a range of current densities from 0.1 to 1.6 A g−1. A Solartron 1470E/1400 potentiostat was used to obtain cyclic voltammetry (CV) curves, and also to perform the electrochemical impedance spectroscopy (EIS) tests that were carried out within a frequency range from 100 kHz to 0.01 Hz. The energy (E) and power density (P) calculation details are explained in Notes S1 and S2.†
Fig. 1a and b show the SEM images of the as-prepared Si/C composite in disk morphology with particle size ranging from 10 to 20 μm. The magnified SEM image and TEM image in Fig. 1c and d show the surface of the main particles which was rough and decorated with a large amount of nanoparticles sizing around 50 nm. The nature of silicon nanoparticles with a 5 nm carbon shell is clearly observed and its crystalline spacing with 0.317 nm corresponds to the silicon crystal (Fig. 1e). Fig. 1f shows the selected area electron diffraction (SAEM) of the center of Si/C which exhibits diffraction rings and light diffraction spots. The content of carbon and silicon in the composite was found to be approximately 92.4 and 7.6 wt%, respectively, based on thermogravimetric (TG) analysis (Fig. S1, ESI†). The large weight percentage of carbon can effectively relieve the stress caused by the volume change of silicon during the charge–discharge processes.
Fig. 1 (a–c) SEM images of the Si/C composite under varied magnifications; (d) TEM image, (e) HR-TEM image and (f) selected area electron diffraction patterns of the Si/C composite. |
Si/C composites were evaluated by half-cell tests against Li metal at potentials between 0.01 and 1.5 V. Fig. 2a presents the first five CV cycles of the half-cell at a scan rate of 0.1 mV s−1. Two peaks located at 0.54 and 0.93 V of the first cathodic scan originated from the formation of a solid electrolyte interface (SEI) on the Si/C. The cathodic peak at 0.12 V originated from the insertion of lithium and the formation of the amorphous LixSi phase (a-Si + xLi → a-LixSi). Meanwhile, an anodic peak at 0.35 V arose due to the extraction of lithium from alloyed Li–Si (a-Lix+ySi → a-LixSi + yLi + ye−). The CV curves almost overlapped in the following four cycles, showing reversible behavior. The rate capability of the Si/C electrode was also tested at varied current densities and the results are shown in Fig. 2b. Reversible capacities of 488.8, 443.9, 389.8, 317.0, 283.0, and 270.5 mA h g−1 were achieved at current densities of 100, 200, 400, 800, 1000, and 1600 mA g−1, respectively, indicating superior capacity and rate capability. After the current density was reset to 100 mA g−1, the cell retained a capacity of 487.1 mA h g−1. Galvanostatic charge and discharge curves were measured at 100 mA g−1 current density and are plotted in Fig. 2c. The galvanostatic curves of the Si/C electrode showed a distinct discharge voltage plateau below 0.3 V, demonstrating that lithium ions had embedded in Si/C particles to form the LixSi alloy and LixC compound. The initial discharge/charge capacities were 553 and 448 mA h g−1, respectively. And the initial coulombic efficiency was 81.1%. The loss of charge capacity was due to the formation of SEI films.46,47 The discharge capacity showed a significant increase within 200 cycles and reached a maximum value of 500 mA h g−1. Such capacity increment was found to be accompanied by the formation of a polymeric gel layer, which came from the degradation of the electrolyte, over the electrode. For long cycling performance at 100 mA g−1 (Fig. 2d), the electrode still delivered a reversible capacity of 449.4 mA h g−1 after 500 cycles, implying outstanding cycling stability.
Fig. 2 (a) CV curves at a scan rate of 0.1 mV s−1, (b) rate performance at varied currents, (c) charge/discharge profiles and (d) long cycling performance at 100 mA g−1 of the Si/C electrode. |
Since the energy density of a hybrid device is determined by both the capacities and the working voltage, the cathode capacity and operating voltage are also of significance. Graphite, which can store anions like PF6− and TFSI− under high operating voltage via intercalation into the interlayer space,37,38 was extensively used as the cathode for dual ion LIBs. It was demonstrated that the storage of PF6− anions into graphite occurs through pseudocapacitive intercalation behavior instead of chemical intercalation behavior. Considering that the ion size of PF6− (4.36 Å) is much larger than the interlayer spacing of graphite layers (3.36 Å), increasing the layer distance may benefit the PF6− anion insertion. In this work, EG, which was prepared according to a previous report,48 was selected as the cathode. Fig. 3a shows the SEM image of the as-prepared EG. EG displayed an interconnected sheet-like morphology and provided a moderate surface area of 90.4 m2 g−1 (Fig. S2, ESI†). EG presented a diffraction peak at 2θ = 26.6° referring to the (002) plane of graphite (Fig. 3b), corresponding to an interlayer distance of 3.46 Å. The value enlarged as compared to that of crystal graphite.
The electrochemical performance of EG for PF6− anion storage was evaluated by galvanostatic charge/discharge measurements at varied currents as shown in Fig. 3c. For comparison, activated carbon (with a surface area of 1768 m2 g−1, Fig. S2, ESI†) was also tested. Three distinct platforms (4.40–4.68, 4.68–4.82 and 4.82–5.00 V) on the charging branch and three platforms (4.97–4.74, 4.74–4.46 and 4.46–4.12 V) on the discharge branch were observed. This suggested that the intercalation and de-intercalation processes occurred via a stage-like mechanism, agreeing well with the previous literature reports.49,50 The rise of current density from 100 to 1600 mA g−1 just caused a modest decrease in the capacity of the EG electrode from 104.1 to 76.7 mA h g−1, implying enhanced electrode reaction kinetics. Note that the AC cathode delivered capacities of only 60.9 and 36.9 mA h g−1 at current densities of 100 and 1600 mA g−1 (Fig. S3a, ESI†). Fig. S3b (ESI†) shows the rate capability of the EG electrode, which was much superior to AC, exhibiting excellent reversible capability. The cycling stability of the EG electrode was also tested at a fixed current density of 100 mA g−1 as shown in Fig. S3c (ESI†). The electrode maintained a high capacity of 96 mA h g−1 after 200 cycles. The energy density of the EG electrode, calculated by the Vm (the midpoint discharge voltage obtained from the discharge curves.) and capacity, ranged from 418.1 to 488 W h kg−1 at power densities of 0.456–9.786 kW kg−1, superior to the 109.4–235.1 W h kg−1 of the AC electrode at 0.378–8.971 kW kg−1 (Fig. S3d, and Note S1, ESI,† which explained the details of the calculations).
To confirm the energy-storage behavior of the EG electrode for PF6− anion storage, cyclic voltammetry (CV) curves were measured using varied sweep rates and the results are shown in Fig. 3d and S5 (ESI†). In general, the peak current (i) could be correlated with the sweep rate (v) viaeqn (1) and (2) as follows:25,45
i = avb | (1) |
log(i) = blog(v) + log(a) | (2) |
i = k1v1/2 + k2v | (3) |
i/v1/2 = k1 + k2v1/2 | (4) |
CV curves of the lithium-based hybrid dual-ion energy storage device (Si/C//EG) were recorded within the potential window of 3.0 to 5.0 V with the results shown in Fig. 4a. Three sets of redox peaks were observed that corresponded to the intercalation/de-intercalation of ions into/from the electrode. Three reduction peaks (3.71, 4.18, and 4.55 V) and the equivalent oxidation peaks (4.37, 4.47, and 4.68 V) of the Si/C//EG cell, which were attributed to the intercalation/de-intercalation of PF6− anions into/from the interlayers of graphite,17 remained visible. Notably, the CV curves retained their shape over the cycles, indicating that electrochemical reactions took place in a highly reversible manner.
The charging/discharging profiles of the Si/C//EG device at a current density of 100 mA g−1 (Fig. 4b) showed three reduction peaks located at approximately 3.70, 4.15 and 4.76 V and corresponding oxidation peaks at approximately 4.40, 4.49 and 4.70 V. These results were consistent with the stage-like potentials on the CV curves. To obtain the rate capability, the hybrid cell was further tested at various current densities from 0.1 to 1.6 A g−1 (Fig. 4c). The cell delivered reversible discharge capacities of 109.7, 106.6, 101.3, 93.4, 89.2, and 77.9 mA h g−1 under 0.1, 0.2, 0.4, 0.8, 1, and 1.6 A g−1, respectively. Note that, after cycling at a current density of 1.6 A g−1, a discharge capacity of 109.4 mA h g−1 was achieved when the current was set back to 0.1 A g−1.
It should be mentioned that the hybrid device suffered from high irreversible charge capacity, originating from the formation of the SEI layer,52 leading to low coulombic efficiency during the original cycles. The device delivered a discharge capacity of 122.7 mA h g−1 under a current of 0.1 A g−1 in the beginning (Fig. 4d). The coulombic efficiency was 66.7% in the first cycle, but the value later increased to more than 90% after 100 cycles under a current density of 0.1 A g−1. After cycling for 500 cycles, the current density was set to 0.5 A g−1. The cell provided a discharge capacity of 96.4 mA h g−1 with coulombic efficiency climbing as high as 97.8%. The Ragone plots of Si/C//EG devices are presented in Fig. 4e. The energy and power densities were calculated based on the total mass of active materials in both the anode and cathode. The maximum energy density reached 252 W h kg−1 at a power density of 215 W kg−1 (the details of the calculation are given in Note S2, ESI†). The Si/C//EG full cell maintained a high energy density of 222.6 W h kg−1 even at a high power density of 5420 W kg−1, demonstrating remarkable energy/power delivery compared with recently reported dual graphite pseudocapacitors (energy densities of 231.7–220.2 W h kg−1 at power densities of 222–4409 W kg−1). This enhanced performance was associated with the fact that the silicon carbon anode provided a higher capacity than the graphite anode, which was more beneficial to improve energy density. The energy/power densities of the Si/C//EG exceed those of benchmark double-ion batteries, supercapacitors, lithium-ion capacitors and pseudocapacitors as reported in the literature (Table S4, ESI†). Since the mass of active electrode materials accounted for 35–40% of the total package,53–55 the Si/C//EG could achieve an energy density comparable to that of a commercial LIB (Fig. 4f). And the power density could also be comparable to that of supercapacitors maintaining an appropriate value.
To gain insight into capacity fading during cycling, electrochemical impedance spectroscopy (EIS) was conducted for the original cell and the cell after 20 and 200 galvanostatic cycles (Fig. 4g). The Nyquist diagram demonstrated a semicircle in the region of high-frequency and a straight line in the region of low-frequency. The high frequency region is controlled by the electrode reaction kinetics, and the low frequency region is controlled by the diffusion of reactants or products of the electrode reaction. During the cycle, repeated intercalation/delamination of ions at the insulating layer caused a certain change in the electrode material interface. This process belongs to electrode reaction kinetics. So it appears in the high-frequency region after cycling. The internal impedance was shown through its equivalent circuit model inset of Fig. 4h and i. In this model, Rs represented the resistance of the electrolyte solution. Wo referred to the Warburg impedance arising from diffusion of ions into the electrodes. The value of Rs was quite low (12.0 Ω), suggesting low resistance in the electrolyte solution. In addition, the two semicircles that emerged in the high-frequency region after cycling corresponded to Rct and Rint paralleled with the constant phase element (CPE), accounting for the charge transfer impedance and the contact impedance, respectively.56 Notably, only a small increase in the impedance was seen (from 40.0 to 60.0 Ω). Thus, the decay in the capacity with cycling may not be due to the deteriorated reaction kinetics, but mainly due to a loss of Si nanospheres from the electrode, suggesting an important influence of the carbon, the binder pitch and the volume buffer on the integrity of the core–shell-like structure of Si nanospheres in the Si/C composite anode.
Multiscale characterization techniques including ex situ XRD, SEM and Raman spectroscopy have been carried out. As shown in Fig. 5, the Si/C electrode after the full cell charging to 5.0 V showed a significant difference in diffraction peaks, which could be attributed to the LixSi alloy during the charging processes, compared with the electrode material before charging (Fig. 5a). Fig. 5b and c show the morphology change of the Si/C before and after cycling under a current density of 500 mA g−1. Before cycling, the Si/C electrode showed a smooth surface. After cycling, the Si/C electrode presented huge erosion/exfoliation on the surface resulting from the alloying/de-alloying reaction causing volume changes.
For the EG electrode, there is no obvious morphology change in the electrode morphology before and after the electrochemical reaction as shown in Fig. 5d and e. Further, ex situ X-ray diffraction (XRD) and Raman spectroscopy had been carried out. The XRD patterns of the EG electrode at certain charge states are presented in Fig. 5f. With the charging potential reaching a value over 4.5 V (vs. Li/Li+), the (002) peak of non-intercalated EG was replaced by two fresh peaks at 23–26° and 30–35°, assigned to the (00n) and (00n + 1) peaks of intercalated EG compounds. Moreover, the emergence of the peak (00n + 1) was a clear indication of the intercalation of PF6− between the layers of EG. When the EG electrode was charged to higher potentials (5.0 V), the (00n) peak shifted gradually to a low angle while the (00n + 1) peak shifted to a high angle, indicating a stage-like intercalation of PF6− (from stage 4 to stage 1 as seen in Fig. S6, and Table S5, ESI†). During discharging, the peaks (00n) and (00n + 1) started to shift gradually in an opposite manner, until the (00n + 1) peak disappeared, and the position of the non-intercalated peak was recovered.49 Comparing these changes to the processes of charging and discharging of the EG cathode, the appearance of the same (00n) peak in the same state indicated that the change in the interlayer distance during charging/discharging took place reversibly, which was in agreement with the results of the electrochemical measurements demonstrated above. Raman spectroscopy measurements were also performed for the EG cathode, shedding light on the intercalation and de-intercalation of PF6− of the electrode (Fig. 5g). The original EG cathode displayed a well-defined G band at 1581 cm−1, attributed to the E2g vibration mode and the bond stretching in the sp2 carbon.50 In the course of charging, the G band changed into a doublet (∼1584 cm−1 attributed to the E2g2(i) mode and ∼1610 cm−1 due to the E2g2(b) mode), due to the electronic effect of the intercalant species and symmetry variation of the boundary EG layer. Concurrently, the peak intensity of the E2g2(b) mode increased with charging, indicating the gaining of PF6− anions intercalating into the EG cathode. During discharging, the two obvious peaks were still observed, which can be induced by the de-intercalation of PF6− anions from the interlayers of EG. With the continuous discharging of the electrode to 3.0 V, the EG returned to its symmetrical structure, showing reversible de-intercalation of the PF6− anion from the EG cathode.
Based on multiscale characterization test results, it could be concluded that the PF6− anions were intercalated/deintercalated into/from EG interlayers during charge/discharge processes and Li+ had formed the LixSi alloy at the Si/C anode electrode.57–59 Therefore, it can be inferred that the overall reaction taking place in the dual-ion hybrid devices (Si/C//EG) may be expressed in the following manner:
Cathode:
nC + (x + y)PF6− ↔ Cn[PF6](x+y) + (x + y)e− | (5) |
Anode:
Si + xLi+ ↔ LixSi − xe−, C + yLi+ ↔ LiyC − ye− | (6) |
Overall:
nC + Si + C + (x + y)PF6− + (x + y)Li+ ↔ Cn[PF6](x+y) + LixSi + LiyC | (7) |
Footnotes |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/c9ta12660k |
‡ These authors contributed equally. |
This journal is © The Royal Society of Chemistry 2020 |