O.
Westhead
ab,
M.
Spry
a,
A.
Bagger
cd,
Z.
Shen
a,
H.
Yadegari
a,
S.
Favero
d,
R.
Tort
d,
M.
Titirici
de,
M. P.
Ryan
ae,
R.
Jervis
ef,
Y.
Katayama
g,
A.
Aguadero
aeh,
A.
Regoutz
i,
A.
Grimaud
*bjk and
I. E. L.
Stephens
*ae
aDepartment of Materials, Imperial College London, UK. E-mail: i.stephens@imperial.ac.uk
bSolid-State Chemistry and Energy Laboratory, UMR8260, CNRS, Collège de France, France. E-mail: alexis.grimaud@bc.edu
cDepartment of Chemistry, University of Copenhagen, Denmark
dDepartment of Chemical Engineering, Imperial College London, UK
eThe Faraday Institution, Quad One, Harwell Science and Innovation Campus, Didcot, OX11 0RA, UK
fEletrochemical Innovation Lab, Department of Chemical Engineering, University College London, UK
gSANKEN, Osaka University, Japan
hInstituto de Ciencia de Materiales de Madrid ICMM-CSIC, Spain
iDepartment of Chemistry, University College London, UK
jRéseau sur le Stockage Electrochimique de l’Energie (RS2E), CNRS FR 3459, 80039 Amiens Cedex 1, France
kDepartment of Chemistry, Merkert Chemistry Center, Boston College, Chestnut Hill, MA, USA
First published on 28th November 2022
Since its verification in 2019, there have been numerous high-profile papers reporting improved efficiency of lithium-mediated electrochemical nitrogen reduction to make ammonia. However, the literature lacks any coherent investigation systematically linking bulk electrolyte properties to electrochemical performance and Solid Electrolyte Interphase (SEI) properties. In this study, we discover that the salt concentration has a remarkable effect on electrolyte stability: at concentrations of 0.6 M LiClO4 and above the electrode potential is stable for at least 12 hours at an applied current density of −2 mA cm−2 at ambient temperature and pressure. Conversely, at the lower concentrations explored in prior studies, the potential required to maintain a given N2 reduction current increased by 8 V within a period of 1 hour under the same conditions. The behaviour is linked more coordination of the salt anion and cation with increasing salt concentration in the electrolyte observed via Raman spectroscopy. Time of flight secondary ion mass spectrometry and X-ray photoelectron spectroscopy reveal a more inorganic, and therefore more stable, SEI layer is formed with increasing salt concentration. A drop in faradaic efficiency for nitrogen reduction is seen at concentrations higher than 0.6 M LiClO4, which is attributed to a combination of a decrease in nitrogen solubility and diffusivity as well as increased SEI conductivity as measured by electrochemical impedance spectroscopy.
10th anniversary statementWe would like to congratulate the Journal of Materials Chemistry A on their 10 year anniversary. The journal has been instrumental in bringing the materials research community together, especially in the fields of energy and sustainability, and has highlighted major breakthroughs in the area. In our paper on electrochemical ammonia synthesis, we utilise the wealth of information on battery science to gain insight into lithium-mediated nitrogen reduction. In particular, we demonstrate the importance of Solid Electrolyte Interphase (SEI) tailoring and understanding, drawing on the recognised effect of salt concentration on SEI stability. We hope that this work, among others, promotes further interdisciplinary investigation with the aim of moving beyond lithium. Prof. Magda Titirici states “It was such a joy and privilege for me to act as an associate editor over the past 10 years, and to see the journal flourish. I have published and reviewed many battery papers in J. Mater. Chem. A, and it is wonderful to be involved in this work translating my battery knowledge to electrocatalysis”. Dr Ifan Stephens states “It is particularly pertinent that our paper is published in J. Mater. Chem. A, as it draws on battery science to understand catalysis; over the past 10 years, the journal has spearheaded high quality research in both fields”. |
A better solution would be one powered by electricity from renewable energy sources operating at ambient temperature and pressure, which would eliminate carbon emissions. Such a solution would also allow for production at the point of use, reducing capital expenditure and global fertiliser inequity.5,8 There has been, therefore, a great deal of interest over the past 30 years in electrochemical nitrogen reduction. Here, N2 gas is reduced on a catalyst surface in the presence of protons to produce ammonia. However, the vast majority of results are false positives.9 It is likely impossible to efficiently reduce nitrogen to ammonia in aqueous electrolytes due to extreme competition with the hydrogen evolution reaction (HER), which can also result in electrode poisoning and deactivation.10,11 The only rigorously verified electrochemical nitrogen reduction paradigm is that pioneered by Tsuneto et al. in the 1990s and later verified by Andersen et al. in 2019.12–14 This is the lithium-mediated nitrogen reduction system, where an organic solvent, non-aqueous proton source and lithium salt work in concert to allow for non-negligible ammonia yields. Since 2019, great steps forward have been taken in system optimisation by considering cell design and choice of lithium salt,3,15–18 proton source choice,13,16,19 N2 partial pressure,13,19,20 potential cycling,20 and oxygen inclusion.21 However, while these advances have resulted in commendable improvements in selectivity, stability and activity, there has been little to no investigation into exactly why the lithium mediated system is able to outperform all other solid-electrode paradigms.22
Most models cite the ability of lithium metal – which is plated on the working electrode in situ – to spontaneously dissociate the highly energetic N2 triple bond as the driving force of the reaction.3,20 However, this strong binding to N2 is accompanied by a stronger binding to protons;23 this is problematic given the requirement of the presence of both N2 and protons to form ammonia. Furthermore, when considering the sole example of efficient, stable and active ambient nitrogen reduction, the enzyme nitrogenase, it is clear that immediate NN scission is not a pre-requisite for ammonia synthesis.24,25 This phenomenon is echoed in homogeneous systems.26,27 The key to the lithium-mediated system could lie in lithium's unique ability to form a Solid Electrolyte Interphase (SEI).22 On the first charging cycle of a Lithium-ion Battery (LiB), electrolyte decomposition products are deposited onto the electrode surface. These form a layer that is electronically insulating but lithium ion conducting, providing kinetic stability to prevent further electrolyte degradation.28 It is the formation of this SEI layer that allows LiBs with graphite anodes to operate for 1000 s of cycles. A similar layer is formed in the lithium-mediated nitrogen reduction paradigm, as evidenced by Electrochemical Impedance Spectroscopy (EIS),29 X-Ray Photoelectron Spectroscopy (XPS) and X-Ray Diffraction (XRD) measurements.21 The SEI layer likely controls the access of protons to the electrode surface, reducing competition with the HER and allowing the system to make ammonia.20,22,30 Herein, we rigorously link bulk electrolyte properties to SEI characteristics to fully understand their impact on the subsequent efficiency of nitrogen reduction, understanding which has thus far been lacking in the literature.
A well-established issue with the electrolyte originally used by Tsuneto et al.,13,14 and since employed by Chorkendorff, Vesborg, Nørskov and coworkers,12,20 is its lack of stability under the required electrochemical conditions. At the beginning of a chronopotentiometry experiment, where a constant current density is applied and the electrode potential measured, the working (negative) electrode sits at lithium plating potentials. However, over the course of the experiment, the working electrode becomes more negative compared to the counter (positive) electrode (Fig. 1a and S6†). This problem is henceforth referred to as ‘working electrode drift’, and results in significantly decreased energy efficiency.18,19 This electrolyte is made of up 0.2 M LiClO4 dissolved in tetrahydrofuran (THF), with an addition of 1% v/v EtOH as a sacrificial proton donor, henceforth referred to as the Tsuneto electrolyte. Clearly this problem and the resulting poor energy efficiency means that the Tsuneto electrolyte is not suitable for any realistic device.
Fig. 1 (a) The change in working electrode (WE, molybdenum foil coated with in situ deposited LixNyHz) stability with LiClO4 concentration. A constant current density of −2 mA cm−2 is applied until −10C is passed. Stability occurs at 0.6 M LiClO4, where the counter electrode (CE, platinum mesh) potential also settles at a lower value. WE and CE potentials reported vs. the observed lithium plating potential and corrected for ohmic losses. A Pt wire is used as a pseudo-reference. The electrolyte is varying concentrations of LiClO4 in THF containing of 1% v/v EtOH as a sacrificial proton donor. Further experimental details can be found in the ESI (Fig. S2–S4†) (b) The change in faradaic efficiency and yield rate with LiClO4 concentration (n = 3 separate experiments, error bar is standard error in the mean) for a chronopotentiometry experiment at an applied constant current of −2 mA cm−2 until −10C is passed. (c) The extended operation of a 0.6 M LiClO4 electrolyte. Potential reported vs. the observed lithium plating potential and corrected for ohmic losses. Two other greyed out traces are shown to indicate the reproducibility of the experiment. −2 mA cm−2 was applied for 12 hours. (d) The change in N2 solubility and diffusivity in THF at different concentrations of LiClO4. Solubility and diffusivity were measured using N2 absorption with a porosity analyser. See ESI section 8 and Fig. S7† for full experimental details. (e) Simulated and experimental Raman spectra of various co-ordination geometries of LiClO4 in THF. Simulated spectra are obtained using Density Functional Theory (DFT). See ESI part 9† for details on DFT calculations. (f) Theoretical Radial Distribution Functions (RDFs) for lithium in 0.5 M, 1 M and 1.5 M LiClO4 concentrations in THF. The RDFs were obtained using ab initio molecular dynamics, as explained in ESI part 9.† (g) Space filling diagrams of LiClO4, THF, ClO4− and the 4THF–Li and 3THF–Li–ClO4 clusters. DFT data set can be found in ref. 31. |
A variety of solutions to the problem of working electrode drift have been presented in the literature, but there has been no clear explanation as to exactly where the problem stems from. Chorkendorff, Vesborg, Nørskov and coworkers addressed working electrode drift by using a potential cycling method, where a short current pulse of 2 mA cm−2 was applied, followed by a period at open circuit potential. Here the authors claim the pulsing technique prevents the build-up of undesired products on the working electrode.20 Suryanto et al. achieved improved stability through electrolyte design, utilising a phosphonium salt as a recyclable proton donor, in place of sacrificial ethanol, and 0.2 M LiBF4 rather than 0.2 M LiClO4, but do not explain the origin of their improved stability.19 Chorkendorff, Vesborg, Nørskov and coworkers21 have also shown that the introduction of small amounts of oxygen into the inlet gas results in greater stability, citing increased SEI homogeneity and decreased Li+ ion diffusion as reasons for higher faradaic efficiency and stability. Du et al. also achieved close to 100% faradaic efficiencies using higher concentrations of LiNTf2 salt under 15 bar N2, suggesting that a thin and dense SEI results in improved Li cycling and faradaic efficiency.17 However, this study did not focus on SEI or bulk electrolyte characterisation. It is also worth stating that the relationship between faradaic efficiency and N2 partial pressure is relatively well understood; the faradaic efficiency increases with increasing N2 partial pressure up to a certain point, after which it no longer improves. Andersen et al. note this point as 10 bar N2 partial pressure.20 Chorkendorff, Nørskov, Vesborg and co-workers recently show that the use of a fluorinated salt results in the formation of a LiF layer, which improves SEI stability and electrochemical performance.18 However, the reason why the Tsuneto electrolyte offers poor stability remains a relative mystery. In this work we seek to fully understand the problem of working electrode drift in relation to bulk electrolyte and SEI properties, as well as to provide further fundamental insight into the mechanisms of lithium mediated nitrogen reduction.
Our initial studies suggest that the SEI formed in the Tsuneto electrolyte may either be unstable or not fully passivating, with decomposition products continuing to be deposited after initial cycling. Time-of-Flight Secondary Ion Mass Spectrometry (ToF-SIMS) data in Fig. S1† shows that the SEI becomes more dominated by heavy, likely organic mass fragments after the electrode potential has been allowed to drift. Such organic species are likely to result from continued solvent decomposition.32 We hypothesise that this increase in organic species results in a more resistive SEI, forcing the electrode to more negative potentials to be able to continue passing the same constant current density. The answer to this issue can be found in battery science.
The electrolytes used in LiBs have been well optimised. The most common choice is a mixture of 1 M LiPF6 in an organic solvent containing a cyclic carbonate, often ethylene carbonate (EC), as an SEI-former, and a linear carbonate, often dimethyl carbonate (DMC), to maintain the optimal physical properties of the electrolyte.33 Several factors govern this choice, one of which is to provide an optimal battery SEI.33 It is important to note, however, that the ideal N2 reduction SEI may differ from the ideal battery SEI.21 The properties of the SEI are primarily tailored by varying the composition of the bulk electrolyte, both via the ratio of solvents used and by the addition of electrolyte additives such as vinylene carbonate (VC) or fluoroethylene carbonate (FEC).34 The SEI is strongly affected by the solvation environment of the Li+ ion, since whatever is contained within the Li+ solvation shell will be preferentially reduced on the electrode on the first charging cycle. If the Li salt is well solvated by the solvent, the solvation shell will be made up of more solvent molecules than salt anions, which will result in an SEI made up primarily of organic solvent decomposition products.32 This is similar to what we see in Fig. S1† when using the Tsuneto electrolyte. However, in the burgeoning field of superconcentrated electrolytes, very high concentrations of lithium salt in an organic solvent can be used to increase the stability of the SEI, especially for lithium-metal batteries.33 This phenomenon is possible since the high concentration of salt increases the lithium salt anion content in the Li+ solvation shell, which creates a SEI layer that is mostly comprised of inorganic salt reduction products.35 These themes from battery science can provide insight for the Li-mediated nitrogen reduction system. Increasing the concentration of salt in the Tsuneto electrolyte could create a more stable, more inorganic SEI and prevent working electrode drift, which was briefly mentioned by Li et al.,36 where the authors noticed an improvement in stability with a 2 M LiClO4 concentration. Until now there has been limited fundamental understanding of exactly how the bulk characteristics of the electrolyte impact the catalytic performance of the system, and even less understanding into the role or chemical makeup of the SEI.
In this paper, we use a model system, the Tsuneto electrolyte under 1 bar N2 partial pressure, to study the effect of increased salt concentration on faradaic efficiency and SEI characteristics in detail. While other studies have made excellent progress in improving stability, faradaic efficiency and activity,18,22 here we seek to gain more fundamental understanding of the exact properties of the bulk electrolyte and SEI which yield the best results. We link bulk electrolyte properties, such as salt solvation and N2 solubility and diffusivity, to SEI characteristics, system stability, ammonia yield and faradaic efficiency using a combination of electrochemical measurements, Density Functional Theory (DFT) calculations, bulk electrolyte characterisation and a variety of advanced post-mortem characterisation techniques.
Interestingly, the counter electrode potential is also affected by the salt concentration. At 0.2 M LiClO4, the potential remains stable at approximately 6 V vs. Li+/Li, whereas the more concentrated samples all have less positive counter electrode potentials at around 4 V vs. Li+/Li.37 The impact of the anode reaction on the lithium-mediated nitrogen system will be the subject of further studies. Fig. S6† shows the change in the DFT-calculated HOMO–LUMO (Highest Occupied Molecular Orbital–Lowest Unoccupied Molecular Orbital) of THF at various concentrations of LiClO4. As LiClO4 concentration increases, the HOMO–LUMO separation decreases. HOMO–LUMO separation is not directly related to electrolyte stability, and instead electrolyte redox potentials should be considered. However, in many cases the redox potentials of non-aqueous solvents are correlated with the HOMO–LUMO gap.39 Therefore, as we increase salt concentration, we may decrease the thermodynamic electrolyte stability by closing the HOMO–LUMO gap, which may partly explain the change in anode potential. However, the formed SEI in the more concentrated electrolytes appears to be more able to kinetically stabilise the system at the cathode due to the observed increase in working electrode stability in Fig. 1a and S5.†
Indeed, we can obtain the limiting current density for nitrogen reduction from the equation
Jlim = nFDN2[N2]δ−1, | (1) |
Fig. 1e shows simulated (labelled DFT) and experimental Raman data for varying concentrations of LiClO4 in THF and different THF–Li–ClO4 environments, shown in space filling diagrams in Fig. 1g. In the experimental 0 M LiClO4 spectrum, we assign the central peak at 913 cm−1 to the C–O stretching frequency of THF.41 As LiClO4 concentration increases, a shoulder is formed to the right of the central THF peak, broadening with increasing concentration to include two peaks at 932 cm−1 and 937 cm−1. Kameda et al. note that the symmetric stretching mode of ClO4− overlaps with the C–O stretching mode of THF and is also strongly affected by interactions with Li+ ions.42,43 This effect causes a shift to higher wavenumbers with increasing interaction, so the shift is weakest for free solvated ions, moderate for Solvent Separated Ion Pairs (SSIPs) and for Contact Ion Pairs (CIPs), and strongest for aggregates.42 SSIPs are a pair of ions separated by a solvent molecule, whereas CIPs are ion pairs not separated by a solvent molecule. Free solvated ions are not connected to another ion at all. There is some confusion in the literature about how to identify the exact solvation environment of lithium perchlorate via Raman spectroscopy. Some authors suggest that the free solvated ClO4− ion peak occurs at around 933 cm−142 and the SSIP peak occurs at between 937 cm−142 and 939 cm−1,41 with the CIP peak forming at around 948 cm−1.43 However, later authors suggest that free solvated ions and SSIPs are spectroscopically identical, and so assigned the peaks at around 939 cm−1 and 948 cm−1 to CIPs and aggregates respectively.43,44 This makes it difficult to determine the exact solvation environment of the Li+ ion. Fig. S8† shows Fourier Transform Infra-Red (FTIR) spectra obtained for varying LiClO4 concentrations in THF. These spectra suggest the formation of more highly coordinated ion environments with increasing salt concentration, with evidence for the presence of both CIPs and aggregates.44 In Fig. 1e, we therefore assign the 932 cm−1 peak to free solvated ClO4− or SSIPs, and the 937 cm−1 peak to more highly coordinated geometries, such as CIPs or aggregates.
The DFT simulated spectra in Fig. 1e of the 4THF–Li and 3THF–Li–ClO4 clusters also show the change in the oxygen–lithium bonding environment, either between oxygen from THF and lithium, or oxygen from ClO4 and lithium. The main peak for 4THF–Li occurs at around 910 cm−1, which may explain the stretching of the central THF peak towards lower wavenumbers due to an increasing lithium concentration. There is a peak at around 930 cm−1 in the simulated 3THF–Li–ClO4 environment that may correspond to fully solvated ClO4− or an SSIP. Whilst the simulated Raman spectra are not a one-to-one match with the experiments on Raman-shift, they do indicate how the Li–ClO4 clusters pair with THF molecules to introduce the additional right-hand peak at higher salt concentrations.
Fig. 1f shows the DFT calculated Radial Distribution Functions (RDF) of a lithium ion in THF with increasing LiClO4 concentration. As LiClO4 concentration increases, it becomes more likely to find an oxygen from the ClO4− anion within the first few angstroms from the lithium. Therefore, as the LiClO4 concentration increases, the average interaction between the oxygen from the ClO4− and Li will get stronger due to increased proximity, resulting in the peaks seen in the experimental Raman data and the formation of more coordinated solvation structures.
Fig. 2 X-ray photoelectron spectroscopy spectra of a Cu working electrode after passing 10C at −2 mA cm−2 under N2 for 0.2 M, 0.6 M and 1 M LiClO4 in 99:1 THF:EtOH electrolyte. All spectra are normalised to the maximum value for that spectrum. Therefore, all intensities are relative rather than absolute. (a) Cl 2p, (b) Li 1s, (c) C 1s, (d) how the relative atomic concentration of O, Li, C and Cl change as electrolyte salt concentration varies according to XPS. The O 1s core level had no clear features (see Fig. S9†). The N 1s core level was too low intensity to be observable. |
Fig. 3 Comparison of the ToF-SIMS traces for the 0.2 M, 0.6 M, and 1 M LiClO4 samples on a Cu working electrode after passing −10C under N2 at −2 mA cm−2. (a–c) Cl species for 0.2, 0.6, and 1 M samples, (d–f) Li species for 0.2, 0.6, and 1 M samples, (g–i) C species for 0.2, 0.6, and 1 M samples and (j–l) N and H species for 0.2, 0.6, and 1 M samples. All traces normalised to total counts point-to-point. The traces are shown from the surface of the SEI (0 μm) to the Cu surface of that sample. Sputtering was done with Ar+ clusters (n = 1159). Depth is estimated using the crater depth and assuming a constant sputter rate. Crater depth was measured using an optical interferometer. Full experimental details can be found in the ESI section 4b.† |
Fig. 4 Time-of-flight secondary ion mass spectrometry depth profiles of a Cu working electrode after passing 10C at −2 mA cm−2 under N2 for 0.2 M, 0.6 M and 1 M LiClO4 in 99:1 THF:EtOH electrolyte. All intensities are normalised to total counts point-to-point. The relative depth parameter represents the depth through the SEI, where 0% is the surface of the sample and 100% is the completed removal of the SEI. The 0.2 M SEI sample was approximately 0.5 μm thick, the 0.6 M SEI sample was approximately 2.8 μm thick and the 1 M SEI sample was approximately 3.3 μm thick. (a) Shows the change in the Li− signal with relative depth, (b) shows the change in Cl− signal with relative depth, (c) shows the change in O− signal with relative depth, and (d) shows the change in C− signal with relative depth. Sputtering was done with Arn+ clusters (n = 1159), which is more gentle than single Ar+ ions. Full experimental details can be found in the ESI section 4b.† |
It is clear from Fig. 2 that the surface chemistry shown in the 0.2 M LiClO4 XPS spectra differs significantly from those of the 0.6 and 1 M samples. The organic contribution is much higher for the 0.2 M sample, shown in Fig. 2c and d, which skews the results for the other core level spectra. This echoes our initial ToF-SIMS data (Fig. S1†) which show that the organic content of the 0.2 M LiClO4 SEI increases with time spent at constant current, likely causing total SEI resistance to increase and the working electrode potential to drift to more negative values. However, is also likely that the SEI morphology differs between the three samples. If the 0.2 M sample is more organic, it is likely to be more porous than the higher concentration samples. This may result in a higher contribution from the outermost layers in XPS. Since the information depth of XPS is only a few nanometres, a larger proportion of the measured signal would be from the very surface rather than inside the SEI in a more porous sample. This increased contribution from the SEI surface for the 0.2 M sample compared to the 0.6 and 1 M samples would cause a higher measured level of total carbon and levels of oxidation and hydroxylation, which can be observed in the possible presence of an LiOH peak in the Li 1s core level of the 0.2 M sample (Fig. 2b). Fig. 2d shows the relative atomic concentration of the four XPS core levels considered. The Li 1s and C 1s core levels decrease compared to the O 1s and Cl 2p core levels with increasing LiClO4 concentration, dramatically between 0.2 and 0.6 M, and then more slowly from 0.6 to 1 M. The dramatic difference between the surface chemistries of the 0.2 M and 0.6 and 1 M samples is in line with what we observe in the electrochemical data; while the 0.2 M sample experiences working electrode drift, the 0.6 M and 1 M samples do not. Preliminary microscopy images (not shown) may also show evidence of a more porous morphology for the 0.2 M SEI. This will be the focus of future work. While we can still draw interesting comparisons between the surface chemistry of the three samples, it is important to keep these caveats in mind.
Fig. 2a shows that the relative LiCl to ClO4 content of the 0.2 M sample is much higher compared to the 0.6 and 1 M samples shown in Fig. 2b and c. This could be due to the presence of LiClO4 on the surface of the SEI from the electrolyte in samples from the more concentrated solutions, which remained despite washing; more highly concentrated electrolytes would result in greater quantities of salt on the electrode surface. It may also be that the washing step removed more of the surface layer for the 0.2 M sample, which could have revealed some more reduced Cl species than for the other samples. Fig. 3a–c show the difference in the relative intensities of the ClOx− fragments through the SEI for each sample. For the 0.2 M sample, the ClOx− fragments sharply decrease in relative intensity with depth, whereas the 0.6 and 1 M samples have a more consistent ClOx− depth profile. This phenomenon can also be explained by considering the Raman spectra and radial distribution functions shown in Fig. 1d and e. As salt concentration is increased, the likelihood of finding the ClO4− anion in the Li+ solvation shell increases. Thus, it becomes likely that the ClO4− anion will penetrate into the SEI more deeply and in greater quantities, along with products related to its decomposition. Therefore, the ClO4− anion and related inorganic decomposition products are more abundant in the SEI formed in more concentrated electrolytes. This likely explains the increase in working electrode stability at higher electrolyte concentrations.34
Although Li 1s core levels are notoriously difficult to fit due to the small chemical shift between different Li species, Fig. 2b shows that, as concentration increases, the Li 1s spectrum becomes more symmetrical and decreases in width. This suggests fewer Li species present at the surface of the SEI with increasing concentration, perhaps leaving only lithium bound to ClOn− species. Additionally, only the 0.2 M sample shows a low binding energy contribution at 54.31 eV in the Li 1s spectrum, possible evidence of the presence of LiOH. We expect that all three samples should contain some LiOH due to reactions with trace water28,45 (Table S2†). Indeed, the ToF-SIMS data in Fig. 3d–f show the presence of an LiOH− fragment in all three samples. This could suggest that the potential oversampling of the surface in XPS of the 0.2 M sample lead to greater signal from the LiOH chemical environment in XPS. However, ToF-SIMS is unable to provide quantitative information, so it is difficult to determine if the amount of LiOH at the surface of the more concentrated samples is enough to be detectable in XPS. It may be that the SEI in the more concentrated electrolytes provides greater protection against reactions between lithium and water. Further investigation is required to confirm this hypothesis.
Fig. 2c shows the C 1s core levels obtained for the three SEI samples. The chemical composition of the carbon species does not change appreciably between samples, but the relative intensity of the signal does decrease (highlighted by the increased noise in the more concentrated samples and Fig. 1d). Indeed, Fig. 3g–i do not reveal any different carbon containing species between the three samples. This is to be expected, since organic SEI components will result from solvent decomposition, which remains constant between the three samples.
Both the XPS and ToF-SIMS data did not reveal the presence of many nitrogen containing species within the limits of detection. The N 1s core level was not detectable in the XPS data, and only three nitrogen containing species were observed in ToF-SIMS: NH−, NO− and CN− (Fig. 3j–l). Critically, no lithium–nitrogen species were observed, such as fragments of a mixed LixNyHz species that were predicted as the catalytically active surface by Schwalbe et al.29 or fragments of Li3N as reported by Li et al.21 The absence of such species may be because a large LixNyHz molecule is likely to be broken up into smaller fragments during ToF-SIMS analysis, or because only negative ions were collected. LiH− and LiH2− are observed (Fig. 3d–f), which may be possible fragments of LixNyHz, but there is not an obvious correlation in relative intensity with any N containing species. Li et al. reported Li3N as a surface but not a bulk species. The authors used a 0.3 M LiClO4 in 99:1 THF:EtOH electrolyte, similar to that used in this study, but operated under 20 bar N2 and at varying O2 concentrations, which may alter the surface chemistry. Since the authors generated a much greater quantity of ammonia when operating under these conditions than in this work, it would make sense that a greater quantity of nitrogen containing species were observable.21 However, from the ToF-SIMS data in our current work in Fig. 3, any nitrogen at the surface of the SEI here is more likely to be some nitrogen containing organic species. It may be that these species form from a reaction between an intermediate of nitrogen reduction and the organic electrolyte; interestingly the CN− trace increases in intensity with depth for all three SEI samples (Fig. 3j–l).
Indeed, the detection of reaction intermediates is likely to be difficult via an ex situ, post-mortem technique. While Li3N is stable in the absence of protons, with a standard Gibbs free energy of formation of −154.8 kJ mol−1,46 in the presence of a proton source it should rapidly decompose to form ammonia.29 LiH is slightly less thermodynamically stable with a standard Gibbs free energy of formation of −68.3 kJ mol−1,47 but is less likely to decompose in the presence of protons, which could explain why we are able to observe the lithium-hydrogen species. Additionally, Fig. 3d–f do not show any evidence of a layer composed solely of lithium. It is likely that any metallic lithium surface would have reacted to form something else. Further in situ, operando experiments will be required to probe the active catalytic site of ammonia production.
Fig. 3a–c show an increase in the relative intensity of the CuCl− and CuCl2− traces with depth through the SEI, suggesting an interaction of the copper electrode with the electrolyte, with the rise in the 1 M sample being steadier than that of the 0.2 and 0.6 M samples. In LiBs, transition metal dissolution in current collectors presents a significant stability issue48 which generally increases with increasing salt concentration.49 It is therefore likely that the more concentrated electrolytes result in a greater level of degradation in the Cu electrode, which could lead to more Cu containing species in the SEI. It is likely that this problem is less severe for the Mo electrodes; Cu creates a native oxide in air which is easily removed under reducing potentials,48 whereas we anticipate that of Mo is kinetically challenging to reduce. Nonetheless, the choice of electrode between Cu and Mo does not seem to greatly affect the faradaic efficiency of the system (Table S1†), and the Cl–Cu traces shown in Fig. 3a–c are, in general, of lower relative intensity than the other Cl containing traces, except for the 0.2 M LiClO4 sample. For this sample, all Cl containing traces are of quite low relative intensity after a depth of about 0.25 μm.
The ToF-SIMS data also show a change in the SEI thickness with salt concentration. By evaluating the time at which the Cu− signal reached a peak (Fig. S10†), it is possible to estimate the thickness of the SEI using the total crater depth through optical interferometry. The 0.2 M, 0.6 M and 1 M LiClO4 SEI samples were approximately 0.5 μm, 2.8 μm, and 3.3 μm thick respectively, assuming a constant rate of sputtering. Note that this assumption does introduce some errors and the sputter rate may not be homogeneous throughout different parts of the SEI and the Cu electrode, and each will have different densities, but it can provide a good guide of the relative thickness of each sample.
Fig. 4 shows the Li−, Cl−, O− and C− traces obtained via ToF-SIMS as representative of the total lithium, chlorine, oxygen and carbon content throughout the SEI. To enable easier comparison between samples, this figure considers relative depth through the SEI as a percentage value, with 0% being the SEI surface and 100% being the surface of the copper electrode. This figure allows us to observe the difference in the depth heterogeneity of the three SEI samples. While the 0.6 M and 1 M LiClO4 samples are clearly more organic towards the surface of the SEI and more chlorinated closer to the copper electrode, the 0.2 M LiClO4 sample is generally more homogeneous throughout the depth of the SEI. Both the 0.6 M and 1 M LiClO4 samples also have decreasing relative oxygen content closer to the copper electrode, whereas the 0.2 M LiClO4 sample oxygen content increases with relative depth through the SEI and then saturates approximately 35% of the way through. This could suggest a greater abundance of more reduced species closer to the electrode surface, such as LiCl, in the more concentrated samples. Indeed, for the 0.6 M LiClO4 sample Fig. 3b shows an increase in the LiCl− trace intensity can be seen closer to the electrode surface, and the O− and Cl− traces correlate well in Fig. 4b and d. It is also interesting to note the decrease in surface Li2CO3 content with increasing salt concentration as shown in Fig. 2b. Indeed, Fig. 3g–i show differing behaviour of the CO3− fragment with depth between the three samples. For the 0.2 M sample, the relative CO3− intensity peaks near the SEI surface before declining and stabilising, whereas for both the 0.6 and 1 M samples, the relative CO3− intensity increases with depth through the SEI.
For the Cl− trace in Fig. 4b, we can observe that relative chlorine content increases with depth for the 1 M sample, decreases with depth for the 0.2 M sample and stays relatively stable with depth for the 0.6 M sample until approximately 66% of the way through the SEI when it sharply increases, then saturates (Fig. 4b). This suggests that most of the chlorine in the 0.2 M sample is likely from residual LiClO4 from the electrolyte on the surface of the SEI. This can be seen clearly in Fig. 3a. The XPS data in Fig. 2a, however, suggests a greater relative quantity of LiCl than LiClO4 at the SEI surface for the 0.2 M sample. However, while the samples were not rinsed for the ToF-SIMS study since we were more interested in bulk information, the samples for XPS were rinsed in 0.1 ml THF to remove dried electrolyte. It may be that the, likely more organic, SEI formed in the 0.2 M LiClO4 electrolyte was more soluble in THF and so some of the surface species were washed away to reveal more reduced lithium-chlorine species. It could also be that, since the 0.2 M sample is in general more homogeneous in composition with depth than the other two, as shown in Fig. 3 and 4, we see a greater relative quantity of reduced species at the surface of the SEI than for the 0.6 and 1 M samples.
Thus, these XPS and ToF-SIMS data suggest an increase in SEI stratification, as well as a possible increase in inorganic species, with salt concentration. This suggests that the model of the SEI in battery literature, which consists of a more organic layer close to the electrolyte and a more inorganic layer close to the electrode,28 also holds for the SEI formed using the modified Tsuneto electrolyte, but only for the more concentrated LiClO4 electrolytes. It also suggests that the more chlorinated layer formed closer to the electrode surface in the 0.6 M and 1 M LiClO4 electrolytes is what allows the electrode to become properly protected against further solvent degradation.
Fig. 5 shows Potentiostatic Electrochemical Impedance Spectroscopy (PEIS) spectra for the 0.2 M, 0.6 M and 1 M LiClO4 samples analysed in the XPS and ToF-SIMS. These spectra were fitted to separate the charge-transfer resistance (RCT) at the SEI-electrolyte interface and the SEI resistance (RSEI), with a methodology adapted from that of Wang et al.50 Both RCT and RSEI decrease with increasing salt concentration. While the exact values of RCT and RSEI are not reproducible, the general trend is (see Table S3†). Given that the SEI thickness appears to increase with increasing salt concentration, this trend fits with faster kinetics with increased salt concentration. Given that the PEIS spectra give us aggregated information about total charge transfer through the SEI, it is difficult to determine the specific change in Li+ ion conductivity with salt concentration. However, both the ToF-SIMS and XPS data in Fig. 2d, 3d–f and 4a show a change in the relative lithium content with increasing salt concentration. While the Li− content continually increases with depth in the 0.2 M sample, the 0.6 M sample exhibits a sharp increase then a plateau and the 1 M sample exhibits no change in relative Li− content. This change in the distribution of Li− in the SEI with increasing LiClO4 content could suggest a change in Li+ conductivity. In addition, recent DFT studies suggest that Li2CO3 and Li2O allow for fast Li+ ion diffusion.51Fig. 3d–i show the presence of LiO2− for all three samples and increased relative CO3− content closer to the electrode surface with increasing LiClO4 concentration. This implies the presence of a range of different Li-environments throughout the SEI which change with changing salt concentration. These observations could suggest increased Li+ ion conduction in the SEI formed in more concentrated electrolytes, but further investigation is required to be certain of this conclusion.
Fig. 5 Potentiostatic electrochemical impedance spectroscopy spectra of the same Cu electrodes examined for Fig. 2–4 at the end of a choronopotentiometry experiment. All spectra were recorded between 200 kHz and 100 mHz at an amplitude of 10 mV about open circuit potential, which is approximately 0 V vs. Li/Li+. In general, the spectra became noisier at lower frequencies so some data points at lower frequencies were omitted. (a) 0.2 M LiClO4 electrolyte, (b) 0.6 M LiClO4 electrolyte, (c) 1 M LiClO4 electrolyte. Fitting parameters shown in ESI Table S3.† |
Chorkendorff, Vesborg, Nørskov and coworkers posit that hindering the transport of Li+ ions to the electrode surface can provide a boost to faradaic efficiency, since more electrons will be involved in making ammonia rather than in Li plating.20,21 Li et al. propose that the inclusion of small quantities of oxygen in their feed gas results in a more homogeneous SEI with reduced Li+ transport capability,21 citing work by Wang et al. which shows that O2 inclusion results in improved battery cyclability but increased SEI resistivity.50 In the case of the current work, the PEIS (Fig. 5) data points to a decrease in SEI resistance with increased salt concentration. This also supports the hypothesis that, as salt concentration increases, the SEI becomes less organic and so less ionically resistive. This has been shown through the decrease in relative carbon content, and increase in relative chlorine content, in the SEI with increasing salt content in the electrolyte. This is observed via XPS (Fig. 2d) and ToF-SIMS (Fig. 3d–i and 4a and b). The increased overall conductivity exhibited by the SEI formed in more concentrated samples may suggest increased Li+ ion conductivity, as well as perhaps an increase in proton mobility, through the SEI. However, the increasing thickness, and perhaps density, may also inhibit the transfer of reactants to the catalytically active surface.52 It may be that the combination of these factors contributes to the change in faradaic efficiency with increasing LiClO4 concentration.
Looking beyond lithium, our study also shows how sensitive the Li-mediated system is to even small perturbations in the LiClO4 concentration. Indeed, as discussed in ESI section 10,† we had many difficulties with very small amounts of LiClO4 contamination which delayed experiments by nearly a year. Had we not known from the work of Andersen et al.12 that the Tsuneto electrolyte could reproducibly make ammonia, we would have discounted LiClO4 altogether. Such findings echo those of Lazouski et al.3 who noted a very sharp peak in optimum ethanol concentration, as well as an optimum purity level for the LiBF4 salt. The community should carefully consider the sensitivity of the system before discounting materials for nitrogen reduction, which may either be contaminated or just slightly outside of the ammonia formation window with the right electrolyte stability, ion transport, nitrogen transport, and chemical potential of protons.
We discuss that the solvation environment of the Li+ ion has a significant impact on the structure of the SEI and the stability of the LiClO4 system. Increasing the Li salt concentration increases the likelihood of finding the salt anion within the Li+ ion solvation shell, which in turn increases the proportion of inorganic species in the SEI resulting from salt decomposition. The increased inorganic content of the SEI results in greater electrochemical stability, but this benefit must be balanced with the lower solubility of N2 gas in the more concentrated electrolyte and increased Li+ ion conductivity in the SEI. The problem of N2 solubility could be mitigated by operating at higher nitrogen partial pressure, or perhaps by using novel locally concentrated electrolytes.53
Importantly, this work represents an interesting battery-science motivated step forward in the optimisation of the lithium-mediated nitrogen reduction system. We have shown that it is possible to favourably tailor the SEI, even using a salt and organic solvent not typically used to promote good SEI formation in LiB science. Other avenues could be the use of battery additives to further tune SEI properties,34 or even drawing inspiration from the hydrophobic, anhydrous environment surrounding the catalytically active centre of nitrogenase54,55 to design an artificial SEI. Such a layer could allow for the field to move away from the requirement for in situ lithium plating which fixes the energy efficiency of the lithium-mediated nitrogen reduction at unfeasibly high values22 and instead rely on an active but much less scarce and expensive transition metal catalyst, such as those proposed by Skúlason et al.10 Such artificial SEI layers have been proposed in lithium-metal56 and lithium-sulfur batteries.57 It even opens the possibility for the use of an aqueous bulk electrolyte. Researchers have proposed that a stable, mostly inorganic SEI could provide improved kinetic stability, even in an aqueous battery.34 While such technologies require more investigation before they can be viable,58 the ability to perform aqueous nitrogen reduction in a much milder potential environment would be revolutionary.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d2ta07686a |