Xing
Xie
a,
Meng
Ye
a,
Liangbing
Hu
b,
Nian
Liu
c,
James R.
McDonough
b,
Wei
Chen
d,
H. N.
Alshareef
d,
Craig S.
Criddle
*a and
Yi
Cui
*b
aDepartment of Civil and Environmental Engineering, Stanford University, Stanford, California 94305, USA. E-mail: ccriddle@stanford.edu; Tel: +1-650-723-9032
bDepartment of Materials Science and Engineering, Stanford University, Stanford, California 94305, USA. E-mail: yicui@stanford.edu; Fax: +1-650-725-4034; Tel: +1-650-723-4613
cDepartment of Chemistry, Stanford University, Stanford, California 94305, USA
dMaterials Science and Engineering, King Abdullah University of Science and Technology (KAUST), Jeddah, Saudi Arabia 23955-6900
First published on 9th September 2011
The materials that are used to make electrodes and their internal structures significantly affect microbial fuel cell (MFC) performance. In this study, we describe a carbon nanotube (CNT)–sponge composite prepared by coating a sponge with CNTs. Compared to the CNT-coated textile electrodes evaluated in prior studies, CNT–sponge electrodes had lower internal resistance, greater stability, more tunable and uniform macroporous structure (pores up to 1 mm in diameter), and improved mechanical properties. The CNT–sponge composite also provided a three-dimensional scaffold that was favorable for microbial colonization and catalytic decoration. Using a batch-fed H-shaped MFC outfitted with CNT–sponge electrodes, an areal power density of 1.24 W m−2 was achieved when treating domestic wastewater. The maximum volumetric power density of a continuously fed plate-shaped MFC was 182 W m−3. To our knowledge, these are the highest values obtained to date for MFCs fed domestic wastewater: 2.5 times the previously reported maximum areal power density and 12 times the previously reported maximum volumetric power density.
Broader contextMicrobial fuel cell (MFC) technologies can potentially address both energy and water quality challenges because they can enable clean energy production while also purifying water. MFC principles have been demonstrated for lab scale devices, but scale-up to real-world applications is limited by power yield and long-term performance. In this paper, we describe a new composite electrode fabricated by coating macroporous sponge (a familiar everyday material) with carbon nanotubes (a well-studied nanomaterial). When fed domestic wastewater, CNT–sponge electrodes achieved superior performance, with maximum volumetric power densities 12 times higher than previously reported values. CNT–sponges can be used as both bio-electrodes and as abiotic electrodes with or without catalyst decoration. |
Electrode materials and their spatial orientation significantly affect MFC performance.9 Materials commonly used include commercially available graphite-based electrodes, such as graphite rods,10graphite discs,5graphite felt,11carbon cloth,12 and carbon paper.13 Use of these materials essentially adopts long-standing design criteria developed for chemical fuel cells and batteries, but neglects the biological role of MFC electrodes as habitat for microbial communities. To satisfy this function, electrode materials should facilitate microbial colonization and attachment, substrate transport to attached microorganisms, removal of waste products, efficient transfer of electrons from the microorganisms to the electrode surface, and efficient collection of current from all regions of the electrode. Modified graphite electrodes14–16 and new composites17–20 confer some of these properties. An open three-dimensional (3D) macroporous structure is desirable because it enables internal colonization and efficient transport of substrates. Length scales and the surface area accessible for colonization are particularly important. Although some new electrode materials are porous, pore diameters are normally less than 10 μm and are easily clogged by microbial growth.17Pores that are too small also hinder substrate transport into the electrode interior, wasting surface area. To increase the specific surface area, one research group21 has fabricated a graphite fiber brush electrode with a high specific surface area (7170–18200 m2 m−3) by winding graphite fibers into a twisted core consisting of two titanium wires, but evidence is lacking that the full surface of these fibers is accessible for microbial colonization. Recently, Chen et al. used electrospinning and solution blowing techniques to make 3D carbon fiber nonwovens but pore sizes for these materials were in the range of microns, so clogging remains a concern for long-term application.22 For MFC electrodes that do not require microbial adhesion (cathodes typically), researchers have focused on reducing capital cost by employing catalytic materials other than precious metals, including activated carbon,23Ni,24Fe,25Co,26Mn,27 and N-doped carbon nanotubes (CNTs).28
Previously, we reported on the fabrication and properties of a CNT–textile bio-electrode. A CNT-coated textile provides an open 3D space for internal colonization with efficient electrolyte transport and an affinitive CNT surface for extracellular electron transfer.29 We also used electrochemical deposition to decorate CNT–textile with platinum nanoparticles for oxygen reduction.30 These CNT–textile electrodes achieved superior performance compared to commercially available carbon cloth electrodes. In this study, we changed the electrode substrate from textile, a random structure comprised of intertwined fibers, to sponge, a periodic and tunable structure whose properties can be controlled by varying different synthetic process conditions. Because sponge offers a continuous 3D surface that is virtually free of interrupted junctions, it can enable useful functionalities that are difficult to obtain with paper or textile. The lack of junctions makes it easier to apply a continuous skin of conductive nanomaterials. As shown in Fig. 1a, the sponge open lattice network enables a continuous 3D CNT coating that reduces internal resistance, connects internal surface area and provides a mechanically stable scaffold for microbial colonization. In the present study, we investigated the performance of conventional MFCs outfitted with CNT–sponge electrodes when fed real domestic wastewater. High current densities and power densities were achieved.
![]() | ||
Fig. 1 Carbon nanotube (CNT)–sponge electrode. (a) Schematic of CNT–sponge showing the macroporous structure and continuous three-dimensional (3D) CNT coating. (b) A sponge cylinder before application of a CNT coating (white) and after (black). (c) Scanning electron microscopy (SEM) image of the CNT–sponge. (d) A bent CNT–sponge strip. (e) A CNT–sponge strip before (∼6 cm long) and after (∼12 cm long) stretching. (f) A CNT–sponge cube before (∼1.2 cm thick) and after (∼0.2 cm thick) compression. (g) A CNT–sponge electrode applied in this study (1 cm × 1 cm × 0.2 cm). |
Plain sponges were coated with CNTs through a simple and scalable dipping and drying process.31,32 The sponge was dipped into a CNT ink, allowing the ink to fill the voids and coat the hydrophilic macroscale pores. It was then allowed to dry at ∼90 °C. The mechanical flexibility of individual CNTs and their strong affinity for the sponge surface enabled formation of a CNT “skin” that conformed to the sponge surface.33 This conformal CNT coating conferred conductivity upon the surface area of the entire matrix and changed the color of the sponge from white to black (Fig. 1b). Because the inside surface of the sponge is continuous in three dimensions, the conformal coating is also continuous in all three dimensions (Fig. 1a). As a solid conducting material, the CNT–sponge achieved a conductance of ∼1 S cm−1, even with a CNT coating of only ∼200 nm thick. The CNT–sponge is thus sufficiently conductive to function as an electrode in small scale applications; for large-scale applications, a current collector could be envisioned if necessary.29 The thin CNT coating did not change the macroporous configuration of the sponge. Fig. 1c shows an SEM image of a CNT–sponge with a pore size range of 300–500 μm and the CNT surface as the inset. Based on density measurements, the porosity is ∼98%. The estimated specific surface area is ∼104 m2 m−3 based on the dimensions of the sponge framework and pore size (Fig. 1c). The CNT-coated sponge preserves the mechanical properties of the uncoated sponge: it is flexible and can be bent arbitrarily to any degree (Fig. 1d). It is also stretchable and compressible. Fig. 1e shows a 6 cm long CNT–sponge strip stretched to ∼12 cm and Fig. 1f shows a 1.2 cm thick CNT–sponge cube compressed to ∼0.2 cm. When the applied forces were released, CNT-coated sponges returned to their original shapes without deformation.
As an electrode in MFCs, CNT–sponge has the same benefits as CNT–textile, including an open macroporous structure for efficient electrolyte transport and a microporous CNT layer for strong electrode–biofilm interaction.29 The CNT–sponge also has other advantages. Its continuous 3D CNT coating prevents interruption of contact between the CNT–textile fibers, resulting in lower internal resistance. Pore diameters are more uniformly distributed and can be tuned during sponge synthesis.34 Tunability over a wide range (up to the millimetre scale) allows the pore size to be optimized for different MFC systems. Larger pores are possible because of the internal framework of the sponge. Finally, unlike the CNT–textile, with its layered structure of the limited thickness, the CNT–sponge is isotropic. The CNT–sponge can be processed into any shapes to fit a range of device configurations, such as cubes, cylinders, or strips.
The CNT–sponges can be used as both bio-electrodes and as abiotic electrodes with or without catalyst decoration. In this study, a pristine CNT–sponge and a platinum (Pt) decorated CNT–sponge were investigated as anodes and cathodes, respectively. Organics were oxidized at the anode, and oxygen was reduced at the cathode. Fig. 1g shows a CNT–sponge electrode ready for assembly.
The CNT–sponge achieved a maximum current density of 2.13 mA cm−2 or 10.63 mA cm−3 in glucose media (1 g L−1) (Fig. 2a). This is 48% higher than that obtained from the CNT–textile under the same conditions (1.44 mA cm−2 or 7.18 mA cm−3).29 After 30 days of steady current output, a piece of the CNT–sponge anode was cut open, and the interior was examined. The open porous structure of the CNT–sponge allowed internal colonization (Fig. 2b and c), and the biofilm did not clog the pores. Fig. 2d shows a single microorganism lying on the CNT surface, and illustrates the connection between microbial nanowires and the CNTs. After changing from a glucose medium to filtered domestic wastewater, the CNT–sponge generated a maximum current of 0.52 mA cm−2 or 2.58 mA cm−3 (Fig. 2a). Lower current generation for domestic wastewater compared to glucose media was expected, and has been reported by others.12,35Fig. 3a shows an SEM image of a CNT–sponge–Pt cathode. The bright lines sketch out the framework of the CNT–sponge, and the dots indicate clusters of Pt nanoparticles (Fig. 3a, the inset). With a low Pt loading of 0.17 mg cm−2 or 0.85 mg cm−3, the CNT–sponge–Pt had high oxygen reduction activity with a current density maximum of 4.79 mA cm−2 or 23.95 mA cm−3 (Fig. 3b). Current generation was negligible when the electrolyte was purged with N2 (Fig. 3b), confirming that the negative current was due to oxygen reduction.
![]() | ||
Fig. 2 Use of a CNT–sponge as a conventional MFC anode. (a) Current generation by the CNT–sponge with a mature biofilm from glucose (1 g L−1) and domestic wastewater (265 ± 21 mg COD L−1). (b and c) Interior SEM images of the CNT–sponge after microbial colonization. (d) A single microorganism lying on the CNT surface, illustrating the strong interaction between the microbial nanowires and CNTs. |
![]() | ||
Fig. 3 Use of a CNT–sponge as a conventional MFC cathode. (a) SEM image of a corner of the CNT–sponge after Pt decoration, with the inset showing clusters of Pt nanoparticles. (b) Current generation from oxygen reduction showing the strong catalytic activity of the CNT–sponge–Pt cathode. |
To investigate the full-cell performance of CNT–sponge electrodes, two MFC configurations were employed with different operating modes: a classic H-shaped MFC (HMFC) in batch mode and a compact plate-shaped MFC (PMFC) in continuous mode. The CNT–sponge electrodes were first evaluated in the HMFCs intermittently fed glucose or wastewater. Fig. 4a and b show typical current generation cycles in glucose and filtered wastewater, respectively. Changes in current tracked changes in COD: anolyte COD decreased from 1035 mg L−1 to 100 mg L−1 (90% removal) for glucose (Fig. 4a) and from 280 mg L−1 to 78 mg L−1 (72% removal) for filtered wastewater (Fig. 4b). A marked change in COD occurred when the COD values were lower than ∼100 mg L−1 in both cases. The residual COD may consist of refractory organics and/or soluble microbial metabolism products that cannot be used for power production. Coulombic efficiencies were 13% for glucose and 7% for wastewater. Maximum power density measurements were performed 10 hours after anolyte replacement. At this point, power generation returned to a steady state, while soluble COD levels remained elevated. As shown in Fig. 4c, the maximum power density generated was 1.99 W m−2 or 0.66 W m−3 for the HMFC fed glucose medium, and 1.24 W m−2 or 0.41 W m−3 for the HMFC fed filtered domestic wastewater.
![]() | ||
Fig. 4 Performance of the H-shaped MFC (HMFC) in batch mode. Typical current generation cycles are shown with decreasing anolyte COD values when the HMFC was intermittently fed with glucose (a) or domestic wastewater (b). (c) Polarization curves of HMFCs show the maximum power densities achieved with glucose and domestic wastewater. |
After three replicated cycles of current generation in the HMFCs, the same CNT–sponge electrodes were moved to the PMFCs. Using a continuous flow of glucose media or domestic wastewater, the PMFCs operated at a steady current output for 300 hours and 120 hours, respectively (Fig. 5a and b). The hydraulic retention times were only 6 minutes for glucose media and 2.4 minutes for domestic wastewater. The effluent COD of the glucose-fed PMFC was 340 ± 80 mg L−1 (a removal efficiency of 67% and a volumetric removal rate of 170 g L−1d−1) while the effluent COD of the PMFC fed filtered domestic wastewater was 91 ± 13 mg L−1 (a removal efficiency of 64% and a volumetric removal rate of 113 g L−1d−1). The coulombic efficiencies were 7% for glucose and 9% for wastewater. Measurements of the maximum power density were made at the end of the experiment. As shown in Fig. 5c, the maximum volumetric power densities achieved were 1.30 W m−2 or 325 W m−3 for glucose and 0.73 W m−2 or 182 W m−3 for domestic wastewater.
![]() | ||
Fig. 5 Performance of the plate-shaped MFC (PMFC) in continuous mode. Current generation and effluent COD values when the PMFC was continuously fed with glucose (a) or domestic wastewater (b). (c) Polarization curves of PMFCs showing the maximum power densities achieved with glucose and domestic wastewater. |
The CNT–sponge electrodes achieved higher areal power densities in the HMFCs than in the PMFCs for both glucose (1.99 W m−2vs. 1.30 W m−2) and wastewater (1.24 W m−2vs. 0.73 W m−2). Possible explanations would include: (1) accumulation of electron mediators in the anode chamber during batch operation, and (2) larger anode chambers within the HMFCs (150 cm3vs. 0.2 cm3) may have enabled growth of more unattached microorganisms capable of electron mediator production or partial degradation of complex substrates into simpler substrates that are in turn used for current generation. By contrast, PMFCs achieved ∼500 times higher volumetric power densities than the HMFCs (325 W m−3vs. 0.66 W m−3 for glucose and 182 W m−3vs. 0.41 W m−3 for wastewater), due to more efficient utilization of space (i.e., a more compact device configuration). The continuous flow in PMFCs improved the accessibility of the CNT–sponge to anolyte, and allowed higher power generation.12 Only a few MFC studies have used authentic domestic wastewater as feed.12,35–39 Compared to these previous studies, MFCs equipped with CNT–sponge electrodes achieved at least 2.5-fold higher areal power densities and 12-fold higher volumetric power densities.
To evaluate long-term MFC performance, we fed a glucose medium to an HMFC equipped with CNT–sponge electrodes for about 1 year. Fig. 6a illustrates the maximum operational power density of the consecutive electricity generation cycles. The power output was stable for the first 5 months then declined after 8 months, possibly due to a shift in microbial community structure. As shown in Fig. 6b, the macropores of the CNT–sponge did not clog after about one year of operation.
![]() | ||
Fig. 6 Long-term performance of the CNT–sponge. (a) Maximum operational power density achieved in consecutive electricity generation cycles of a glucose-fed HMFC in batch mode. Power density changes for each cycle reflected the pattern for current density illustrated in Fig. 4a. (b) SEM image of the interior CNT–sponge anode after about one year of operation. |
This journal is © The Royal Society of Chemistry 2012 |