Marta
Oriola
a,
Alenka
Možir
b,
Paul
Garside
c,
Gema
Campo
a,
Anna
Nualart-Torroja
a,
Irene
Civil
d,
Marianne
Odlyha
e,
May
Cassar
f and
Matija
Strlič
*f
aConservation Section, Facultat de Belles Arts, Universitat de Barcelona (UB), C/Pau Gargallo, 4, 08028 Barcelona, Spain. E-mail: martaoriola@ub.edu
bUniversity of Ljubljana, Faculty of Chemistry and Chemical Technology, Aškerčeva 5, SI-1000 Ljubljana, Slovenia
cConservation Research, The British Library, 96 Euston Road, London NW1 2DB, UK
dConservation Department, Fundació Gala-Salvador Dalí, Pujada del Castell, 28, 17600 Figueres, Spain. E-mail: irenecivil@fundaciodali.org
eSchool of Biological and Chemical Sciences, Birkbeck College, University of London, Malet Street, Bloomsbury, London WC1E 7HX, UK
fUniversity College London, Centre for Sustainable Heritage, The Bartlett School of Graduate Studies, 14 Upper Woburn Place, London WC1H 0NN, London, UK. E-mail: m.strlic@ucl.ac.uk
First published on 12th September 2013
A new analytical method was developed to non-destructively determine pH and degree of polymerisation (DP) of cellulose in fibres in 19th–20th century painting canvases, and to identify the fibre type: cotton, linen, hemp, ramie or jute. The method is based on NIR spectroscopy and multivariate data analysis, while for calibration and validation a reference collection of 199 historical canvas samples was used. The reference collection was analysed destructively using microscopy and chemical analytical methods. Partial least squares regression was used to build quantitative methods to determine pH and DP, and linear discriminant analysis was used to determine the fibre type. To interpret the obtained chemical information, an expert assessment panel developed a categorisation system to discriminate between canvases that may not be fit to withstand excessive mechanical stress, e.g. transportation. The limiting DP for this category was found to be 600. With the new method and categorisation system, canvases of 12 Dalí paintings from the Fundació Gala-Salvador Dalí (Figueres, Spain) were non-destructively analysed for pH, DP and fibre type, and their fitness determined, which informs conservation recommendations. The study demonstrates that collection-wide canvas condition surveys can be performed efficiently and non-destructively, which could significantly improve collection management.
Due to the desire and pressure to exhibit iconic works of art, their material state and fitness to withstand handling and travel needs to be assessed. In doing so, chemical and mechanical analysis of the constituent materials of paintings is of vital importance, however, easel paintings are among the most heterogeneous works of art and an analysis of their condition is not a straightforward analytical task. Paintings are layered structures and some compounds can easily migrate from one layer to another.1 While most analytical effort is understandably dedicated to paint layers carrying the aesthetic message, surprisingly few methods exist for characterisation of their structural support, i.e. the canvas, and none are suitable for use on unique masterpieces due to their destructive nature.
Traditionally, canvas has been made of natural fibres such as linen, hemp, ramie, cotton and jute.2 These cellulosic materials are known to be sensitive to acidity of their macromolecular environment, as acids accelerate the rate of hydrolysis of glycosidic bonds in cellulose.3 Using surface water in the natural preparation of fibres leads to the macromolecular environment in the final product being neutral to slightly alkaline, which is beneficial for the stability of untreated canvas. However, application of the primer, paint, glues, and absorption of acidic gases from the environment leads to acidification of the material. Since most of these processes are heterogeneously distributed across a painted canvas, degradation proceeds in a highly heterogeneous manner and significant local differences are possible. A decrease in cellulose molecular weight (or degree of polymerisation – DP) has been shown to result in a decrease in the mechanical properties of paper4 and canvas.5 However, for painting canvases, no quantitative comparison between canvas quality and DP/pH exists, which would make it possible to interpret analytical results (the state of a material) in terms of conservation condition6 of a piece of canvas. At present, the latter can only be performed empirically,7 as degraded canvases are generally discoloured and have low flexibility, at which point a costly conservation intervention may already be required.
In addition to the two chemical properties crucial for the chemical and mechanical stability of canvas, it is also important to know the fibre type used in canvas production. Namely, the raw material importantly influences the hygrothermal response of a canvas, which is of key importance when interventions are considered.
Several methods have found use in studies of hygrothermal/mechanical properties of real painting canvases, among which particularly electronic speckle pattern interferometry8,9 and uniaxial and biaxial tensile testing10,11 have led to a detailed understanding of how the structural properties of a painting support and of the applied paint layers affect the properties of the composite material. Richardson et al.12 reviewed a number of further analytical techniques for non-destructive canvas and textile analysis, including polarised ATR FTIR, spectra of which have been shown to reflect mechanical strength of silk fibres.13 However, many of these techniques require sampling and/or laboratory-based analytical techniques.
For extremely valuable objects, such as Dalí's masterpieces, destructive sampling is not an option, and development of analytical methods enabling collection managers to assess the condition of objects can only be carried out non-destructively. Near-infrared (NIR) spectroscopy in the region 1100–2500 nm in conjunction with multivariate analysis has been shown as a particularly useful technique in characterisation of artwork supports, both for spot analysis14,15 and as an imaging application.16 It is non-destructive (and could also be classified as non-invasive), it requires no sample preparation and can be used outside the typical laboratory environment without compromising the quality of analytical data. The NIR region is of particular interest also because it reflects combination and higher harmonic oscillations of C–H, N–H, C–O and other similar bonds, mainly present in organic materials.17 However, since individual peaks strongly overlap, multivariate data analytical techniques are necessary to extract useful chemical information.18
Among these techniques, partial least square regression (PLS) is of particular interest,12,14–16,19 as it is possible to correlate spectral information with the information obtained by reference analytical methods, thus developing quantitative predictive models that can be used on similar, but unknown samples. If qualitative data is available, classification of samples is often attempted using discriminant analysis (DA), where spectra are classified based on their similarity into defined sample classes.20 Again, the method can be used in a predictive manner to classify similar, but unknown samples. For PLS and DA to yield reasonably successful predictions, high quality of the reference analytical data and validation are essential.
Significant research has been carried out on silk samples, showing that tensile strength of can be modelled using NIR/PLS.12,21 In this work, we attempted to develop PLS models using real historic canvases, hence substantial sampling for the purpose of mechanical testing was not an option. Therefore, methods were developed for determination of pH and DP of painting canvases, and based on the analysis of an extended collection of historical canvas samples, PLS and DA methods were developed using NIR spectroscopy for non-destructive determination of acidity, DP, and fibre composition of a collection of paintings by Salvador Dalí from the Fundació Gala-Salvador Dalí from Figueres, Spain. A highly interdisciplinary method of interpretation of the analytical data was also developed to provide meaningful results to those entrusted with care for the unique masterpieces.
DP0.85 = 1.1[η]. |
Several methods of sample preparation were tested, as viscometry has not been used for determination of the DP of such a variety of real canvas samples before. If present, the primer layer was manually removed, following which the samples were soaked and washed to remove gelatine, dried and defibred. The DP of 95 samples was determined.
(1) Very fragile canvas, it cannot be re-stretched without reinforcement.
(2) Fragile canvas, re-stretching might lead to tearing.
(3) Somewhat fragile canvas, re-stretching can be done carefully.
(4) Canvas in good condition.
In the context of paintings transportation for exhibitions, it would not be advisable to loan those in the first category, since the canvas may not be able to withstand vibrations that transportation implies.
To produce a larger variety of DP values for this part of the study, a number of canvas samples were degraded at 90 °C, 65% RH (Vötsch VC 0020).
Different backgrounds were used during collection of spectra of samples, depending on what was assessed as safe by conservators: a spectralon 99% reflective standard (Labsphere, North Sutton, NH, also used as a white reference for instrument calibration) or several layers of pure cellulose paper. In some cases, no background was allowed if the paint layer was considered to be fragile. Therefore, testing was necessary to ensure that different backgrounds did not affect the quality of spectra and thus the modelled results. This was done using three sample canvases from the reference collection, three paintings from the Conservation Section of the University of Barcelona, and four paintings from the Dalí collection. The modelled pH and DP values obtained from spectra with different backgrounds were compared and the standard deviation of 3–5 measurements was always less than the error of prediction, leading to the conclusion that the background has no statistically significant influence on the modelled result. This is not surprising since it was estimated that the depth from which radiation is reflected and information is obtained, is ca. 0.5 mm14, and all canvases are thicker than that. During measurements, relative humidity of the environment was 40–65%.
Three NIR spectra were collected per analysed spot and averaged using GRAMS 8.0 software (Thermo Scientific) to reduce the sampling error.
Several algorithms were used to analyse experimental results: PLS (partial least squares regression), DA (discriminant analysis) and Mahalanobis distance function (MDF).27,28 The PLS spectral decomposition technique29 was used to correlate pH and DP of canvases with NIR spectra (Grams 8.0). Separate calibration models were generated for each property. Various spectral pre-treatments were used, although multiplicative scatter correction (MSC) for reduction of the scatter effect, standard normal variate (SNV) with detrending, and differentiation using Gap algorithm (1st derivative)30,31 produced the most satisfactory results. Optimisation of the calibration process was achieved using the leave-one-out cross validation procedure and corresponded to the number of latent factors resulting in the lowest root mean squared error of cross validation (RMSECV). The model accuracy was assessed separately using the root mean squared error of prediction (RMSEP) with a validation set of samples separate from the calibration set.
To test whether the spectrum of an unknown sample (painting) was sufficiently similar to the spectra of the reference collection to give predictions of acceptable accuracy, we used PCA/MDF.32 The method combines PCA scores and spectral residuals, and uses them for Mahalanobis group matrix calculations. By including the sum squared spectral residual as a discriminating factor, the maximum allowed variation was set, which is important in the application of the PLS method to Dalí canvases, as this way outliers could be identified, for which the predictions were considered to be too unreliable.
To predict the fibre identity in Dalí canvases, which is of importance to conservation interventions, DA20 was used (XLSTAT, Addinsoft). Using this method, linear combinations of variables (spectral data) are sought for, which separate classes of objects into cotton, hemp, linen, ramie, or jute-containing, or combinations of these. The spectral region used was 1000–2250 nm. All predictor variables were considered to be of equal weight. For each Dalí painting, predictions were calculated for several analysed spots assuming that the whole canvas was of a uniform composition. It was established that two subsequent DA stages were necessary: in the first stage cotton, jute, bast (i.e. all except jute) fibres and combinations of these were distinguished. In the second stage, the samples identified as bast fibres were analysed to distinguish between linen, hemp, ramie and combinations of these.
Furthermore, Principle Component analysis (PCA) was used (XLSTAT, Addinsoft) to visualise the analytical data modelled for Dalí canvases (fibre ID, pH and DP), and painting date, to look for correlations between these parameters.
FGSD Reg. no. | Date | Image | Title and observations on the canvas |
---|---|---|---|
a thought to be a later copy, although signed as 1947. | |||
0020 | 1924 | Siphon with Small Bottle of Rum (Cubist Painting) Canvas with a large stained area at the bottom due to a past conservation treatment | |
0023 | 1926 | Self-Portrait Splitting into Three Canvas with stains due to migration of adhesives/varnishes applied to the paint layer | |
0335 | 1926 | Barcelona Mannequin Painted on the reverse side and some areas left unpainted, therefore canvas exposed to the light | |
0369 | 1935 | Figure and Drapery in a Landscape Canvas homogeneous | |
0336 | 1938 | The Image Disappears Canvas with discoloured areas, reasons unknown | |
0378 | 1945 | Napoleon's Nose, Transformed into a Pregnant Woman, Strolling His Shadow with Melancholia amongst Original Ruins Darker areas due to the preparation procedure | |
0053 | 1947a | Backdrop for the Ballet "Labyrinth" | |
0340 | 1947 | Dematerialization Near the Nose of Nero Canvas homogeneous | |
0058 | 1954 | Gala Contemplating the Corpus Hypercubicus Canvas with stained areas | |
0372 | 1955 | Portrait of Laurence Olivier in the Role of Richard III Canvas with discoloured darker areas due to the preparation procedure, and with stains of unknown origin | |
0066 | 1960 | Gala Seen from Behind Looking in an Invisible Mirror Half of the canvas of a darker colour due to the preparation procedure | |
0071 | c.1968 | Study for The Hallucinogenic Toreador Canvas with darker areas due to the preparation procedure |
In fibre analysis, it turned out that 2 canvases contained synthetic fibres, so that their classification as outliers was justified from the point of view of fibre content. More samples were available for pH determination since the reference method requires a smaller sample than for DP determination, hence different sample sets used.
For the PLS method of pH determination, the best validation results were obtained by mean-centring of spectra, followed by 1st derivation (Gap, 9 points), standard normal variate detrending, and 9 factors were used. For the DP method, the spectra were mean centred, followed by 1st derivation (Gap, 11 points) and standard normal variate detrending, with 14 factors. Also, this method gave better results if the water peak was disregarded, so the spectral region used in PLS regression consisted of 1200–1870 and 2000–2250 nm, which was different to the pH PLS method, which made use of the full spectral interval.
The developed PLS methods (Fig. 1) indicate that there are satisfactory correlations between modelled and measured values. The RMSEP values of ±0.43 pH units and ±275 DP units were to be expected, given that historical canvases not only contain the already heterogeneous natural textile impregnated with natural glue, but often also primer, oil and varnish penetrating from the upper layers of the painting. The RMSEP value of 0.43 pH units is comparable with the measurement uncertainty of the reference method, which is 0.3 pH units.
Viscometric DP determination is an accurate method with a typical uncertainty of <1%, although for heterogeneous historic canvas samples, typical measurement uncertainties for triplicate determinations were up to 10%, while the standard error of prediction of 275 represents approximately ∼20% uncertainty in the middle range of DP values. The uncertainties of PLS methods are thus only approximately twice as high as the corresponding uncertainties of the reference methods, which is considered to be successful given the significant heterogeneity of samples.
On the basis of the reference set of samples analysed for fibre content, two-stage linear discriminant analysis was performed using spectral data in the interval 1500–2250 nm. In the first stage, separation between ‘cotton’, ‘bast’ (hemp, linen, ramie, or linen and hemp), ‘jute’ (also a bast fibre but can be confidently identified using microscopy) and ‘combinations’ (jute and cotton, jute and ‘bast’, ‘bast’ and cotton) was attempted.
Namely, warp and weft threads were sometimes made of different fibres, and sometimes threads made of a mixture of fibres were used, in which case the measured NIR spectrum would represent a mixture of individual spectra of the two fibre types, as the measurement spot was Ø2 mm. Several such mixed-thread canvases were determined. To build the method 113 samples were used, and 60 were used for validation. In the second stage, only the ‘bast’ category fibres were taken into account from the first stage, 73 to build the method and 38 to validate it. These were grouped into four further categories: ‘linen’, ‘hemp’, ‘ramie’ and ‘combination’ of linen and hemp.
A very satisfactory separation into the three easily identifiable main groups of natural fibres was obtained (Fig. 2, top), which is probably based on the fact that cotton, jute and bast fibres can easily be differentiated using an optical microscope. According to the confusion matrix (Table 2), cotton and also bast (linen, hemp or ramie) samples can be classified with high confidence, while the less populated groups of jute and combination fibres are classified 50–67% correctly. Not surprisingly, combination fibres can be classified as either pure fibre as well. Undoubtedly, the reason for the less successful classification of these fibres is the fact that there were only a small number of canvases available made of jute and combinations jute/cotton, jute/linen, linen/cotton and hemp/cotton.
Known | Classified as | Total | % correct | |||
---|---|---|---|---|---|---|
B | Cb | Ct | J | |||
Stage 1 | ||||||
Estimation | ||||||
B | 72 | 0 | 1 | 0 | 73 | 99% |
Cb | 0 | 4 | 1 | 0 | 5 | 80% |
Ct | 0 | 0 | 30 | 0 | 30 | 100% |
J | 0 | 0 | 0 | 5 | 5 | 100% |
Total | 72 | 4 | 32 | 5 | 113 | 98% |
Validation | ||||||
B | 35 | 0 | 3 | 0 | 38 | 92% |
Cb | 0 | 2 | 1 | 1 | 4 | 50% |
Ct | 0 | 0 | 15 | 0 | 15 | 100% |
J | 1 | 0 | 0 | 2 | 3 | 67% |
Total | 36 | 2 | 19 | 3 | 60 | 90% |
Known | Classified as | Total | % correct | |||
---|---|---|---|---|---|---|
Cb | H | L | R | |||
Stage 2 | ||||||
Estimation | ||||||
Cb | 1 | 0 | 2 | 0 | 3 | 33% |
H | 0 | 5 | 0 | 0 | 5 | 100% |
L | 0 | 0 | 58 | 0 | 58 | 100% |
R | 0 | 0 | 4 | 3 | 7 | 43% |
Total | 1 | 5 | 64 | 3 | 73 | 92% |
Validation | ||||||
Cb | 0 | 0 | 2 | 1 | 3 | 0% |
H | 0 | 2 | 1 | 0 | 3 | 67% |
L | 2 | 2 | 21 | 3 | 28 | 75% |
R | 0 | 1 | 2 | 1 | 4 | 25% |
Total | 2 | 5 | 26 | 5 | 38 | 63% |
In the second phase, sub-grouping of samples identified as ‘bast’ in the first phase was attempted (Fig. 2, bottom). Considering that it is often difficult to reliably identify the individual fibre types in this group and considering that most of the bast canvases were made of linen, the lower success of the second-stage DA is not surprising. None of the combinations were correctly identified, while identification of linen and hemp was reasonably successful. To increase the success of the second stage DA, more of reliably identified hemp and ramie canvases would be needed.
It needs to be stressed that the validity of the developed NIR methods is limited to canvases that are similar to those in the reference collection, i.e. mainly 19th and 20th-Century canvases, with no synthetic fibres, and with a primer layer. The validity of the method has not been tested for extremely soiled or mould-infested canvases and it is likely that the PLS and DA methods would not give reliable results for such materials.
Reg. no | Sampling area | pH | DP | Fibre ID1 | Fibre ID2 | Date |
---|---|---|---|---|---|---|
0020 | Canvas (n = 5) | 5.7 | n/a | Ct (100%) | — | 1924 |
Stained area (n = 4) | 5.8 | n/a | ||||
0023 | Canvas (n = 3) | 5.7 | 550 | Ct (64%), B (36%) | — | 1926 |
Stained area no. 1 (n = 3) | 5.7 | 350 | ||||
Stained area no. 2 (n = 3) | 5.5 | 700 | ||||
0335 | Canvas (n = 4) | 5.3 | n/a | Ct (100%) | — | 1926 |
0369 | Canvas (n = 15) | 5.1 | 1500 | B (51%), J (44%) | L (98%), R (2%) | 1935 |
0336 | Canvas (n = 15) | 5.2 | 800 | B (100%) | L (78%), R (22%) | 1938 |
Discoloured area (n = 3) | 5.0 | 750 | ||||
0378 | Canvas (n = 15) | 5.2 | 800 | B (100%) | L (99%), R (1%) | 1945 |
Discoloured area (n = 3) | 5.2 | 600 | ||||
Stained area (n = 1) | 5.2 | 300 | ||||
0053 | Canvas (n = 4) | 6.7 | n/a | Ct (100%) | — | 1947 |
0340 | Canvas (n = 15) | 5.6 | 1000 | B (100%) | R (52%), L (48%) | 1947 |
0058 | Canvas (n = 6) | 5.7 | 1030 | B (100%) | L (90%), R (10%) | 1954 |
Stained area (n = 2) | 5.7 | 1300 | ||||
0372 | Canvas (n = 3) | 5.4 | 1150 | B (100%) | L (99%), R (1%) | 1955 |
Discoloured area (n = 3) | 5.3 | 1050 | ||||
Stained area (n = 3) | 5.4 | 850 | ||||
0066 | Canvas (n = 3) | 5.8 | 1400 | B (100%) | L (94%), R (6%) | 1960 |
Discoloured area (n = 3) | 5.8 | 1200 | ||||
0071 | Canvas (n = 3) | 6.0 | 1350 | B (100%) | L (99%), R (1%) | 1968 |
Discoloured area (n = 3) | 5.7 | 1150 | ||||
Stained area (n = 1) | 5.9 | 1350 |
The data in Table 3 indicates clearly identifiable differences between the canvases. In the first-step DA, most canvases have been identified as ‘cotton’ or ‘bast’ (i.e. bast fibres except jute) with considerable certainty (Table 2). Only two canvases represent uncertain cases: for Reg. no. 0023 there is a significant possibility for the material not to be cotton, which might indicate the possibility of the canvas being a combination of cotton and bast fibres, although the possibility of a combined-fibre canvas was not flagged up at this stage. Reg. no. 0369 is another example of uncertain identification, the canvas could be either ‘bast’ or ‘jute’ (or a combination). Since there was a slightly higher possibility for this canvas to be of a ‘bast’ fibre, this canvas was also analysed in the second-stage DA.
Jute canvases are probably the only ones that can be quite confidently identified by visual observation. Similarly, when canvases have one of the threads made of jute, the difference between the warp and the weft can easily be spotted with the naked eye. Finally, whereas hemp and linen or cotton and synthetic fibres have traditionally been mixed to produce “mixed threads”, we have not come across any canvas where jute fibres have been mixed with other fibres to produce such mixed threads. For all these reasons, it is likely that there is probably no jute present in Reg. no. 0369 and that it is indeed a linen canvas, as the second-stage DA indicates. On top of this, a commercial Lucient Lefebvre–Foinet stamp was identified on the reverse of this painting in the course of this research (reading “Toiles & Couleurs/Extrafines/Lucien Lefebvre–Foinet/Paris/19, Rue Vavin & 2, Rue Brèa”), which would indicate the canvas is a good quality linen support from the well-established French artists' materials company (this painting has the highest DP value of all: 1500, despite its age). This perfectly corresponds with the period when Dalí was living in Paris, when he would get his materials in French local shops.34
The second-stage DA method clearly exhibits difficulties in discriminating between linen and ramie, as also indicated by the confusion matrix (Table 2), where in the validation phase most misidentified ramie fibres were classified as linen and some also vice versa. It is therefore reasonable to expect to have similar difficulties with the real canvases. Samples, which were identified as linen with less than 90% probability are Reg. no. 0340, which could be either ramie or linen, and Reg. no. 0336, which is most probably linen. It is worth stressing again that microscopic identification of ramie fibres is itself uncertain, which is why DA should be interpreted with caution.
Looking at the oil paintings (i.e. disregarding Reg. no. 0053, which is a 9 × 13 m theatre backdrop, 1947), the three that are painted on cotton (the cheapest support to paint on) are all from Dalí's student days in Madrid (1922–1926). In his maturity, he is known for having always sought good quality materials (i.e. linen supports)34 and so the use of cotton in the early days can be linked to the very experimental period of the young artist.35 Dalí returns to using cheap cotton supports only in his very last days, after Gala's passing and the person in charge of supplies seemed not to care as much about their quality.34
The acidity of canvases is not significantly different, except for one almost neutral and thus stable canvas (pH 6.7), and Reg. no. 0336, which has a local area that is significantly more acidic than other (pH 5.0). These results are in line with the canvas pH values found in other paintings analysed.36 Increased acidity is a significant problem for long-term preservation of canvases due to decreased chemical stability of cellulose.3
However, there are significant differences in the DP. From among the non-stained canvases, there is one, which is particularly degraded (DP < 600), Reg. no. 0023. Three others (Reg. nos. 0336, 0378 and 0340) have midrange DP values (600–1000), while the majority are in a very good condition with DP values >1000. Six of the analysed paintings had stains on the canvas caused by oil, varnish or adhesives, which were also analysed to see if the canvas was more degraded in these areas. In half of the instances this was actually the case, while in other cases the stains may have protected the base material.
On the other hand, five of the analysed Dalí paintings were found to have discoloured darker canvas areas that were thought to be the result of the application of an industrial preparation layer since they tended to follow a regular pattern (broad darker and lighter stripes, Fig. 3). In all these paintings, the discoloured darker areas had a lower DP than in the non-discoloured areas, which would indicate that migration of components present in the preparation layers, such as oils, might have promoted the degradation of canvas.
Univariate analysis of the available data (Table 3) may not reveal any useful correlations, as the parameters (age, pH, DP, fibre ID) could be co-dependent. In Fig. 4, the loading plot is shown for PCA performed on the data in Table 3. PC1 generally separates according to extent of degradation, with the samples with better material properties (higher DP and pH) having more positive values. The loading plot reveals that higher DP values are associated with younger canvases, confirming that ageing of canvases results in lower DP. There is a weak indication that canvases with higher pH have higher DP, and that bast fibres are generally in a better state; however, due to the small number of non-bast samples and generally similar pH values of the canvases, it is difficult to expect strong correlations. On the other hand, the narrow distribution of pH values of the analysed canvases (Table 3) could also indicate that past environmental conditions, particularly acidic pollutants, might have played a role.
Fig. 4 Loading plot for PCA of the data in Table 3 for all Dalí paintings (n = 11). Fibre ID as a descriptive parameter was modeled using the value of 0 for cotton and 1 for bast (linen or ramie). |
However, while scientific analysis is of high importance in the understanding of the material state of canvases, analytical data need to be expertly interpreted in order to assess whether there is a correlation between the analytically determined material state, and the conservation condition of a canvas.
While most attention is given to the integrity of the paint layer carrying the aesthetic information, the structural element, i.e. canvas, is only visually assessed for evidence of existing damage. Material characterisation methods allowing collection managers to assess the magnitude of risk of damage during loans would thus be very welcome. While acidity and fibre type are unlikely to play an important role in such assessments, it is known that for certain fibre types, DP strongly correlates with mechanical properties.38
Thus, a test was designed to investigate the correlation between DP and canvas condition, as assessed by a panel of 17 independent experts. Given the uncertainty of subjective categorisation, a surprising correlation between condition categories and DP was obtained (Fig. 5). The categories are broadly defined, which is reflected in the uncertainty; however, the uncertainty of DP prediction is comparatively small, which enables us to define categories on the basis of DP.
Undoubtedly, there are other parameters defining canvas mechanical properties, such as glue content, but given that the number of reference samples was significant and highly variable in terms of material composition, the influence of glue is evidently of lesser importance. On the other hand, the strength and adhesion of the primer and paint layers must also have an effect; however, these need to be assessed using structural assessment methods, e.g. holography.39
Data in Fig. 5 reveal that canvases with DP < 600 were mostly classified into category “Very fragile canvas”, where excessive stress is not advised due to risk of physical damage. This is higher than the value 250–300, which is usually taken as the value at which paper loses all mechanical strength,40 and DP 400 which is considered to be the value at which historic paper containing iron gall ink is considered at risk.15 It is possible that in canvases better quality of fibres are required to perform the mechanical operations required to tack a canvas onto the stretcher.
Looking at the Dalí canvases in Table 3, we see that only one painting could be categorised as very fragile (Reg. no. 0023), while such low DP values could also be found in the stains of this same painting and of Reg. no. 0378, meaning these two paintings have locally significantly degraded areas. The other paintings are all in a good condition, and can safely continue to be enjoyed by Dalí enthusiasts.
• The developed PLS methods for the prediction of the canvas pH and DP are considered to be very satisfactory given the heterogeneity of the samples, with RMSEP values ±0.43 units for pH and ±275 units for DP.
• A two-stage DA method was developed, the first-stage DA reliably distinguishing between ‘cotton’, ‘jute’ and the rest of the ‘bast’ fibres (linen, hemp, ramie or linen and hemp). The second-stage DA further distinguishes between ‘bast’ fibres, and is less reliable probably due to the fact that there are only a few hemp, ramie and linen and hemp samples available in the reference sample collection.
• A categorisation method was developed with a panel of experts, defining the ‘Very fragile’ category as the category of paintings so weak that they would not withstand canvas manipulation, such as re-stretching without tearing, and thus no longer fit for travelling either. Despite the uncertainty of subjective tests, a surprising correlation between the condition categories and DP was obtained, with the threshold DP for the ‘Very fragile’ category being 600.
• Using the non-destructive methods based on NIR spectroscopy, the pH of all the Dalí canvases was found to be between 5.0 and 6.7, while most of the canvases had DP > 1000, and only one painting with DP < 600, i.e. in the ‘Very fragile’ category.
• PCA performed with the analytical data obtained for the Dalí canvases revealed that DP decreases with age, and indicated that lower pH might accelerate the degradation process, and that cotton canvases possibly degrade faster than linen ones.
It is of interest that Dalí used the less expensive cotton canvases in the early days of his career when he was a student, and replaced them for the higher quality linen supports when his work gained recognition.
While this research was performed using a number of real canvas samples (199), most were of a geographically and temporally limited origin. To improve the applicability of the method, it would need to be validated a broader sample set of different provenance and age. The new method, involving the development and optimisation of destructive methods of chemical analysis, NIR methods, and methods of data interpretation presented here enables curators and conservators to survey the condition of painting collections and base collection management on evidence, with data obtained in an efficient and non-destructive manner. If in further studies, dose–response functions are developed for degradation of painting canvases, modelling of future degradation and predictive maintenance could be enabled.
This journal is © The Royal Society of Chemistry 2014 |