Masaaki
Sadakiyo
*ab,
Teppei
Yamada‡
a,
Kenichi
Kato
c,
Masaki
Takata
c and
Hiroshi
Kitagawa
*ad
aDivision of Chemistry, Graduate School of Science, Kyoto University, Kitashirakawa-Oiwakecho, Sakyo-ku, Kyoto 606-8502, Japan. E-mail: kitagawa@kuchem.kyoto-u.ac.jp
bInternational Institute for Carbon-Neutral Energy Research (WPI-I2CNER), Kyushu University, 744 Moto-oka, Nishi-ku, Fukuoka 819-0395, Japan
cRIKEN SPring-8 Center, 1-1-1 Kouto, Sayo-cho, Sayo-gun, Hyogo 679-5148, Japan
dCore Research for Evolutional Science and Technology (CREST), Japan Science and Technology Agency (JST), 7 Goban-cho, Chiyoda-ku, Tokyo 102-0076, Japan
First published on 5th November 2015
Closed–open structural transformations in flexible metal–organic frameworks (MOFs) are of interest for potential applications such as separation, because of their complete selectivity for the adsorption of specific guest molecules. Here, we report the control of the adsorption behaviour in a series of flexible MOFs, (H2dab)[M2(ox)3] (H2dab = 1,4-diammoniumbutane, M = Fe, Co, Ni, Zn, or Mg), having different central metals with analogous crystal structures. We found that a significant change in the selective adsorption behaviour for EtOH over MeCHO and MeCN is caused by the type of central metals, without changes in the crystal structures of all phases (except the Ni compound). A systematic study of adsorption measurements and structural analyses of the analogous MOFs reveals for the first time that the framework flexibility around the central metals of MOFs is truly related to the selective adsorption behaviour.
We have focused on controlling the selective adsorption behaviour of flexible MOFs that exhibit closed–open structural transformations by means of the difference in the type of central metals in a series of homologous frameworks. We believe that the type of central metals is an important parameter for controlling selective adsorption behaviour because it fine-tunes the energetics of the framework distortion during the adsorption/desorption process. Thus far, some MOFs that show no closed–open behaviour have been investigated for the ability to control adsorption properties through the type of central metals.26–30 For example, a series of inflexible M2(dobdc) (dobdc = 2,5-dioxido-1,4-benzenedicarboxylate, M = Mg, Mn, Fe, Co, Ni, and Zn) MOFs has been reported to show different adsorption behaviours for various gases.26 However, they did not show significant changes in selective adsorption behaviours because of the rigid framework of the M2(dobdc). We believe that a significant change in selective adsorption behaviour could be created in flexible MOFs that show closed–open structural transformations through using different types of central metals, as some research indicates that structural changes in flexible MOFs could be affected by the type of central metals.31–33 However, significant control of selective adsorption behaviour through the type of central metals, such as adsorption or non-adsorption, has not been observed in homologous frameworks, although an example of TCNQ-based MOFs that contain Zn2+ and Mn2+ ions and have different structures in the guest-free condition has been reported.34 Thus, the effect of the type of central metals on the adsorption properties of isostructural flexible MOFs that show closed–open transformations has not been sufficiently clarified to date.
Here, we report a systematic study on the effect of the type of central metals on the selective adsorption behaviour of MOFs that show closed–open structural transformations. We employed an oxalate-bridged layered MOF (H2dab)[Zn2(ox)3]·nH2O (abbreviated to Zn·nH2O, H2dab = 1,4-diammoniumbutane, ox = oxalate), that shows a closed–open structural transformation during its adsorption process (Fig. 1a and b).35 This MOF has both hydrogen bond donor (–NH3+) and acceptor (ox2−) sites in the interlayer space; therefore, it can selectively adsorb hydroxyl-functionalized guest molecules such as H2O, MeOH, and EtOH over other guests. This MOF was the first material to show complete adsorption selectivity for the large polar guest EtOH over the smaller polar aprotic guests MeCN and MeCHO.35 We synthesised a series of MOFs, (H2dab)[M2(ox)3]·nH2O (M = Fe, Co, Ni, Zn, and Mg), having different central metals with almost analogous crystal structures. The guest-free anhydrate states, M, also have analogous structures with the exception of the Ni analogue. A systematic study of the adsorption properties of the analogous MOFs reveals that selective adsorption behaviour for EtOH over other guests in the MOF is significantly changed by the type of central metals.
Fig. 1 Representation of the crystal structure of M·6H2O. (a) Honeycomb-shaped layer framework and (b) layered structure of Zn·6H2O.35 (c) Honeycomb-shaped layer framework and (d) layered structure of Fe·6H2O. (e) Honeycomb-shaped layer framework and (f) layered structure of Mg·6H2O. Water molecules are omitted. The grey, red, green, blue, brown, and yellow colours correspond to carbon, oxygen, nitrogen, zinc, iron, and magnesium atoms, respectively. |
To determine the structures of these MOFs, single-crystal X-ray diffraction (SCXRD) measurements were performed. The crystal structures of Fe·6H2O, Zn·6H2O and Mg·6H2O were successfully determined, and the crystallographic data are shown in Tables 1 and S1–S2.† We previously reported the structure of Zn·6H2O.35 The crystal structures of Fe·6H2O and Mg·6H2O were solved using the same space group (P21/n) as that for Zn·6H2O. As shown in Fig. 1, there was no apparent difference in the framework structure among the crystals. Fe·6H2O and Mg·6H2O also formed the typical honeycomb-shaped layer framework consisting of [M2(ox)3]2−, which incorporated H2dab2+ ions in the voids as counter cations. The guest water molecules were trapped in the space between the layers. Fig. 2 shows the guest arrangements and the configuration of hydrogen bonds in the interlayer space. The guest water molecules, the oxygen atoms of the ox2− anions, and the ammonium groups of H2dab2+ are located in the interlayer space and interacted through hydrogen bonds. As is the case with Zn·6H2O, the guest water molecules were strongly trapped both by the hydrogen bond donor (–NH3+) and acceptor (O atoms on ox2−) sites of the host through three types of hydrogen bonds. One site was between water and the hydrogen bond donor sites of –NH3+; another site was between water and the hydrogen bond acceptor sites of ox2− ions; and the third site was between neighboring water molecules. Each water molecule formed two hydrogen bonds with both hydrogen bond donor and accepter sites. It should be noted that the guest arrangements and configuration of the hydrogen bonds in Fe·6H2O and Mg·6H2O were approximately the same as those in Zn·6H2O, meaning that the central metals were successfully changed to other elements without significant distortion of the crystal structures. Single crystals of Co·nH2O and Ni·nH2O could not be obtained in this synthesis; however, as shown in Fig. 3, the Co compound shows a similar X-ray powder diffraction (XRPD) pattern to the hexahydrate under humidified conditions, confirming the existence of a hexahydrate Co·6H2O phase that is isostructural with Fe·6H2O, Mg·6H2O and Zn·6H2O. Note that the Ni·nH2O compound only showed the dihydrate XRPD pattern even under humidified conditions, indicating that there is no Ni·6H2O phase, as mentioned below.
Fe·6H2O | Zn·6H2O | Mg·6H2O | ||||
---|---|---|---|---|---|---|
Formula | C10H26N2O18Fe2 | C10H26N2O18Zn2 | C10H26N2O18Mg2 | |||
Formula weight (g mol−1) | 574.03 | 593.07 | 510.95 | |||
Crystal system | Monoclinic | Monoclinic | Monoclinic | |||
Space group | P21/n (no. 14) | P21/n (no. 14) | P21/n (no. 14) | |||
Unit cell dimensions (Å, deg.) | a = 8.2586(9) | a = 8.3007(8) | a = 8.292(2) | |||
b = 15.864(2) | β = 113.190(1) | b = 15.660(2) | β = 114.592(1) | b = 15.688(4) | β = 114.800(1) | |
c = 9.421(1) | c = 9.3885(9) | c = 9.380(3) | ||||
Volume (Å) | 1134.5(2) | 1109.7(2) | 1107.6(5) | |||
Z | 2 | 2 | 2 | |||
Calcd density (g cm−3) | 1.680 | 1.775 | 1.532 | |||
Crystal size (mm3) | 0.30 × 0.25 × 0.08 | 0.25 × 0.25 × 0.05 | 0.30 × 0.30 × 0.05 | |||
Temperature (K) | 100 | 100 | 113 | |||
Wave length (Å) | 0.71073 (Mo-Kα) | |||||
Theta range (deg.) | 2.57–28.76 | 2.60–28.64 | 3.00–27.48 | |||
Reflection collected | 6475 | 12521 | 8052 | |||
Unique data/parameters | 2699/198 | 2711/197 | 2446/146 | |||
R 1/wR2 (I > 2σ(I)) | 0.0196/0.0529 | 0.0169/0.0460 | 0.0613/0.1980 | |||
R 1/wR2 (all data) | 0.0205/0.0535 | 0.0175/0.0463 | 0.0839/0.2502 | |||
GOF | 1.048 | 1.054 | 1.178 | |||
μ (mm−1) | 1.364 | 2.248 | 0.196 |
Fig. 2 Comparison of the guest arrangements and hydrogen bonds in M·6H2O (M = (a) Zn,35 (b) Fe, and (c) Mg). The grey, red, green, blue, brown, and yellow colours correspond to carbon, oxygen, nitrogen, zinc, iron, and magnesium atoms, respectively. The light blue dotted lines denote the hydrogen bonds around the guests. |
Fig. 3 XRPD pattern of the hexahydrate of (a) Zn·6H2O (simulation)35 and (b) Co·6H2O. |
To characterize the hydrated phases and the thermal stabilities of these samples, thermogravimetric analysis (TGA) was performed under nitrogen gas flow. Fig. S1 (ESI†) shows TG curves of air-dried samples of M·nH2O (M = Fe, Co, Ni, Zn, and Mg), which showed three-step weight loss at RT, 100–120 °C and 300–350 °C. Considering the chemical compositions of the samples and the temperature regions of the weight losses, the weight losses around RT and 100–120 °C can be attributed to the desorption of included water guests. The mass loss at 100–120 °C corresponded to the desorption of two water molecules per formula unit, indicating the existence of the M·2H2O dihydrate phase. According to the SCXRD measurement results, it was clear that the transformation from M·6H2O to M·2H2O easily occurred at around room temperature and that there are three different hydrated phases consisting of M·6H2O, M·2H2O and anhydrate M. Note that the Ni compound did not show any weight loss around room temperature, suggesting that it did not have a stoichiometric M·6H2O phase but only M·2H2O and M phases, which was consistent with the XRPD measurement. The weight losses at approximately 300–350 °C were attributed to the decomposition of ox2− ligands and H2dab2+, indicating that the framework of (H2dab)[M2(ox)3] can stably exist below 300 °C.
The crystal structure of Zn·2H2O was successfully determined using SCXRD. As reported in the literature,35 the crystal structure of the dihydrate is different from that of the hexahydrate (Fig. S2†). In the dihydrate, the guest water molecules were also bound by the hydrogen bond donor and acceptor sites of the host; however, the Zn·2H2O had horizontal 2-D layers, whereas the Zn·6H2O had distorted 2-D layers, indicating that there was a distortion process that occurred during the desorption process.
Fig. 4a shows the water vapor adsorption/desorption isotherms, in which all of the samples except the Ni analogue showed two-step hysteric adsorption/desorption isotherms. The first adsorption step below 0.15 P/P0 corresponded to two water molecules, which was attributed to the stoichiometric hydration of M to form M·2H2O. This step confirmed that all of the samples had a dihydrate phase of M·2H2O, as evidenced by the TGA results. Fe, Co, Zn, and Mg showed additional adsorption of four more water molecules at higher humidity (approximately 0.8 P/P0), which was attributed to the transformation from M·2H2O to M·6H2O. This result indicated that these samples have three stoichiometric phases: anhydrate, dihydrate, and hexahydrate. Only the Ni did not show any additional adsorption in the high humidity region and only had anhydrate and dihydrate phases. In the case of MeOH adsorption (Fig. 4b), all of the samples showed a large amount of MeOH vapor adsorption with gate-opening isotherms. The amount adsorbed corresponded to four MeOH molecules per formula, indicating a stoichiometric phase of M·4MeOH. None of the materials showed a significant change in selective adsorption behaviour, such as non-adsorption of MeOH; however, they showed a clear difference in the gate-opening pressure, which seemed to arise from the type of metal atom. Fe and Mg showed higher gate-opening pressures than Zn, and Ni and Co showed lower pressures.
Fig. 4 Comparison of adsorption/desorption isotherms of Fe, Co, Ni, Zn,35 and Mg for (a) H2O, (b) MeOH and (c) EtOH at 298 K. Brown, red, green, blue, and orange colours correspond to Fe, Co, Ni, Zn, and Mg, respectively. Filled and open symbols indicate adsorption and desorption isotherms, respectively. |
In contrast with MeOH adsorption, there was a significant difference in the EtOH adsorption behaviour. Fig. 4c shows the adsorption/desorption isotherms for EtOH vapor. Co, Ni and Zn showed a large amount of EtOH adsorption, which corresponded to three EtOH molecules with typical gate-opening isotherms, whereas Fe and Mg did not show any apparent EtOH adsorption. This result clearly showed that the difference in the type of central metals caused a significant change in the selective adsorption behaviour for EtOH, resulting in the significant control of EtOH adsorption. As discussed below in the XRPD study, this significant change in the selective adsorption behaviour was purely due to the difference in the framework flexibility as a result of the difference in the type of central metals because these samples have the same crystal structures in all phases (M, M·2H2O, M·6H2O, M·4MeOH and M·3EtOH), except in the case of Ni. This work is the first systematic study demonstrating the control of selective adsorption behaviour through the type of central metals using flexible MOFs that show closed–open structural transformations. As discussed below, we believe that the difference in adsorption behaviour was derived from the covalent character of the Zn2+ and Co2+ ions which make the framework more flexible during the adsorption process.
Fig. 5 shows the adsorption isotherms for all of the guests. All of the samples did not show significant adsorption of N2, MeCN, MeCHO, Me2CO, i-PrOH, n-PrOH and n-BuOH. Almost no adsorption of N2 (77 K) indicated that the anhydrate phases did not have any apparent microporosity, which confirmed that the adsorption processes for H2O, MeOH and EtOH are attributable to closed–open adsorption behaviour. As we previously reported, Zn has excellent hydroxyl group recognition properties, particularly, a non-size selective adsorption for polar protic guests (EtOH over MeCN and MeCHO).35 Considering that Co, Ni, and Zn did not show any adsorption for aprotic guests such as MeCN and MeCHO despite the fact that these molecules are smaller than EtOH, the Co and Ni also displayed hydroxyl group recognition. All of the samples did not adsorb guest molecules larger than EtOH (i-PrOH, n-PrOH, and n-BuOH), indicating that a size limit of included guest molecules exists.
Fig. 5 Adsorption/desorption isotherms of (a) Fe, (b) Co, (c) Ni, (d) Zn,35 and (e) Mg for H2O, MeOH, EtOH, MeCN and MeCHO (288 K), Me2CO, i-PrOH, n-PrOH, n-BuOH and N2 (77 K) at 298 K. |
To clarify the structural transformation during the adsorption processes of these samples, XRPD measurements were performed under various environmental conditions: vacuum (for M), exposure to water (approx. 0.5 and 1 P/P0 for M·2H2O and M·6H2O), methanol (approx. 1 P/P0 for M·4MeOH) and ethanol (approx. 1 P/P0 for M·3EtOH). The samples were placed inside a sealed glass capillary, dehydrated by heating at 80 °C overnight and then exposed to the desired guests. The XRPD patterns under these conditions and the cell parameter refinement results by fitting using the Pawley or Le Bail methods are shown in Fig. S3–S11 and Tables S4–S7 (ESI†). As shown in Fig. S3,† the anhydrate phases of Fe, Co, Mg, and Zn showed similar patterns, which were all successfully fitted to the same unit cell with a P21/c space group (Fig. S4, Table S4†), confirming that they had the same structure. Fe showed some additional peaks below 5° that could not be fitted by this unit cell. We believe that the diffraction peaks were derived from some superlattice structure of the Fe compound, but not from impurities because these peaks also show changes due to exposure to guests (Fig. S5, S7, and S9†). Only the Ni showed a different pattern, indicating that it had a different crystal structure in the anhydrate phase. In the case of M·2H2O (Fig. S5†), all of the compounds showed XRPD patterns similar to the Zn·2H2O, indicating that the difference in the type of central metals did not cause significant structural changes in the dihydrate state, as was the case with the hexahydrate phases discussed above. These dihydrate patterns were successfully fitted to the same unit cell with a space group of P (Fig. S6, Table S5†), which was different from that of M, confirming that the adsorption process from M to M·2H2O included a structural transformation. Note that an additional peak existed below 5° in Fe·2H2O, which was likely derived from the superlattice structure. As evidenced in the SCXRD results, the hexahydrate phases of the samples showed XRPD patterns similar to Zn·6H2O (Fig. S7†). The superlattice peaks of the Fe compound disappeared in the hexahydrate phase. These patterns were well fitted using the space group P21/n (Fig. S8, Table S6†), which was different from the anhydrate and dihydrate, showing that the water adsorption process included two different structural transformations. It should also be noted that there is no prior report of a series of MOFs having different central metals with such structural similarity for each phase during a gate-opening adsorption process, although an example of analogous TCNQ-based MOFs that contain Zn2+ and Mn2+ ions and have amorphous structures in the guest-free condition has been reported.34
Fig. S9† shows the XRPD patterns of M·4MeOH. We previously succeeded in determining the crystal structure of Zn·4MeOH (Fig. S12†).35 The XRPD patterns were fitted using the same unit cell having a P space group (Fig. S10, Table S7†). This result showed that the same structural transformation process existed from M to M·4MeOH during MeOH adsorption for all of the analogues, with the exception of the Ni compound. This result was consistent with the adsorption measurement results, which showed typical closed–open hysteric adsorption isotherms. Considering that the Fe, Mg, Co, and Zn compounds had isostructural M and M·4MeOH phases, the difference in the gate-opening pressure was derived from the difference in the framework flexibility during the adsorption process. This result implied that the host frameworks of Co and Zn were more flexible than Fe and Mg during the adsorption process. In the case of the Ni compound, the framework flexibility cannot be discussed in the same manner as the other compounds because it had a different crystal structure in its anhydrate phase of Ni. However, to compare the gate-opening pressure, we can hypothesize that the summation of the energy loss due to the structural transformation and the energy gain due to the hydrogen bond formation in Ni compound were similar to those in the Co compound. In the case of M·3EtOH, the Co, Ni, and Zn compounds showed almost the same XRPD patterns, indicating that they were also isostructural after EtOH adsorption (Fig. S11†). The patterns were similar to those of M·4MeOH and different from M. Clearly, the adsorption process from M to M·3EtOH included an apparent structural transformation, which was similar to the transformation of M to M·4MeOH. From these results, we could summarize the structural transformations and the difference in selective adsorption behaviours among the homologous MOFs as in Fig. 6. Considering the fact that Fe and Mg, which were estimated to have lower flexibilities in this transformation, did not show any apparent adsorption of EtOH, we can conclude that the significant change in the selective adsorption behaviour for EtOH through the type of central metals was caused by the change in the framework flexibility. To the best of our knowledge, this is the first report proving that the selective adsorption behaviour of MOFs that show closed–open structural transformations can be controlled by controlling their flexibility through the type of central metals. We next investigated which parameters of the metal ions contributed to the control of the adsorption behaviour. Fe2+ and Mg2+ ions (in case of no EtOH adsorption) could not be distinguished from Zn2+ and Co2+ ions (EtOH adsorption) by the order of the fundamental parameters, such as ionic radius (Fe2+ (0.78 Å for octahedral coordination) > Co2+ (0.75 Å) > Zn2+ (0.74 Å) > Mg2+ (0.72 Å)), average bond length of M–O (Fe2+ (2.121 Å in M·6H2O) > Zn2+ (2.087 Å) > Mg2+ (2.075 Å)), and cell volume (Fe (448.9 Å3 per formula (see Table S4†)) > Co (444.7 Å3) > Mg (443.2 Å3) > Zn (442.5 Å3)). However, these ions can be distinguished by the order of the complex formation constants (β1 and β2) for the ox2− ligand (Co2+ (logβ1 = 3.33, logβ2 = 6.20) ≥ Zn2+ (logβ1 = 3.42, logβ2 = 6.16) > Fe2+ (logβ1 = 3.05, logβ2 = 5.15) > Mg2+ (logβ1 = 2.18, no data for logβ2)),45 implying that the significant change in adsorption behaviour was related to the chemical bond between the central metal ions and the ox2− ligands. According to the value of ionic potentials (≡ ion charge divided by ionic radius) of these samples (Mg2+ (2.78) > Zn2+ (2.70) > Co2+ (2.67) > Fe2+ (2.56)), Mg2+ has a strongest electrostatic interaction to oxalate ions. However, Mg2+ has a lower complex formation constant for the ox2− ligands than Zn2+ and Co2+, indicating that there is a high contribution of covalent character of Zn2+ and Co2+ to the chemical bond with ox2− ligands. We believe that the covalent character of the Co2+ and Zn2+ ions tended to allow a slight deformation of the surrounding ox2− ions during the gate-open adsorption process, making Zn and Co more flexible than Mg and Fe. We also believe that the significant control of selective adsorption behaviour through the type of central metals in this compound was realised because of the existence of framework distortion in the honeycomb layer of [M2(ox)3]2−, as was the case for our compound. [M2(ox)3]n− sometimes forms undulating layered structures accompanied by framework distortion (e.g., M·6H2O)46 but normally shows a flattened framework (e.g., M·2H2O).47–49 The difference in the type of central metals seemed to cause differences in the ease of such framework distortion. This type of slight change in the framework structure during the adsorption process might be necessary for achieving the significant change in selective adsorption behaviour.
Fig. 6 A schematic illustration of the difference in the adsorption behaviour among the homologous Fe, Co, Zn, and Mg. |
Footnotes |
† Electronic supplementary information (ESI) available. CCDC 1422201 and 1422202. For ESI and crystallographic data in CIF or other electronic format see DOI: 10.1039/c5sc03325j |
‡ Present address: Center for Molecular Systems (CMS), Department of Chemistry and Biochemistry, Graduate School of Engineering, Kyushu University, Moto-oka 744, Nishi-ku, Fukuoka, 819-0395, Japan. |
This journal is © The Royal Society of Chemistry 2016 |