Cell adhesion is regulated by the mechanical characteristics of the cell environment. The influences of different parameters of the adhesive substrates are convoluted in the cell response leading to questions on the underlying mechanisms, like biochemical signaling on the level of adhesion molecules, or viscoelastic properties of substrates and cell. By a time-resolved analysis of traction force generation during early cell adhesion, we wanted to elucidate the contributions of substrate mechanics to the adhesion process, in particular the impact of substrate elasticity and the molecular friction of adhesion ligands on the substrate surface. Both parameters were independently adjusted by (i) an elastic polyacrylamide hydrogel of variable crosslinking degree and (ii) a thin polymer coating of the hydrogel surface controlling the affinity (and the correlated substrate–ligand friction) of the adhesion ligand fibronectin. Our analysis showed two sequential regimes of considerable force generation, whose occurrence was found to be independent of substrate properties. The first regime is characterized by spreading of the cell and a succeeding force increase. After spreading cells enter the second regime with saturated forces. Substrate elasticity and viscosity, namely hydrogel elasticity and ligand affinity, were both found to affect the kinetics and absolute levels of traction force quantities. A faster increase and a higher saturation level of traction forces were observed for a higher substrate stiffness and a higher ligand affinity. The results complement recent modeling approaches on the evolution of forces in cell spreading and contribute to a better understanding of the dynamics of cell adhesion on viscoelastic substrates.
In this context it is known that cell size and shape are important factors controlling the force generation of adherent cells.2,17–20 Early cell adhesion has been intensely studied to reveal common features of cell spreading.21 Different phases of cell spreading were distinguished in correlation with distinct processes within the adhesion apparatus.22,23 The first contact of the cell and the flattening of the cell body are governed by membrane tension and the underlying actin cortex.23–27 It was shown that the initiation of fast spreading by cell protrusions formed by actin polymerization is dependent on the ligand density of the cell culture substrates.24 For the rate of spreading there are different findings. One report demonstrated a universal principle for a lot of cell types and substrate conditions.21 Other studies showed the cell spreading rate to depend on ligand density or substrate stiffness.5,28–31 In particular Nisenholz et al.31 showed that a detailed understanding of the mechanisms correlating cell spreading with traction force evolution is still missing. With the formation of primary small adhesion sites, nascent adhesions, by cell adhesion receptors of the integrin family, cells start to apply increasing forces to the substrate.28 On the other hand it is also known that resistive forces from the substrate are necessary for the formation of adhesion sites.15 At later stages of cell spreading, the increase of adhesive area slows down and cells start to polarize.23,32 At this stage nascent adhesions mature to large focal adhesions and a contractile actin cytoskeleton is developed.2,28,32 Recent findings support the tight sequence of spreading, traction force generation and adhesion formation.33
During the last decade much evidence has been gathered of a stiffness dependent force generation of cells. Traction force microscopy allows for the assignment of traction forces down to the scale of single focal adhesions.34,35 Growth dynamics and corresponding forces of adhesion sites could be resolved on the time scale of seconds.36 In this context, it has been reported that even small nascent adhesions are able to exert considerable forces.37–39 In contrast, other studies state that force magnitude depends linearly on adhesion area, while traction stress correlates with substrate stiffness.40
On the cell level there is an ongoing discussion how the overall cellular traction force is regulated depending on ECM parameters.30,41 The force balance on the cellular length scale and the state of the contractile actin cytoskeleton – and not the force balance at single adhesion sites – are considered as the regulating factors for force homeostasis of cells.20,33,40,42,43 However, the multitude of influencing parameters, including substrate viscoelasticity, ligand density and arrangement, cell type and their limited observation in a single experiment, led to various partly contradicting results and interpretations.13,19,20,44,45 In particular, viscous contributions, like friction at the cell–substrate interface, were hardly addressed up to now, although their impact on cellular traction forces was shown.13 Two very recent studies addressed the importance and options to investigate the friction between the cell surface and the surrounding support.31,46 Hence it is expected that a closer look on the dynamics of traction force generation depending on controlled viscous and elastic properties of the cell culture substrate will help to better understand the underlying mechanisms.
In this study, we addressed this topic by investigating the early cell spreading and the congruent generation of cell traction forces depending on substrate stiffness and ligand affinity, the latter being correlated with a sliding friction of adhesion ligands.14 Within the first 2 h of cell adhesion of human umbilical cord vein endothelial cells (HUVECs), different regimes of spreading and traction force generation could be revealed. In addition to an elasticity dependent traction force response, an additive effect of the ligand affinity on the force generation was found, in agreement with our earlier findings.13,14 Our results agree with recent experimental and theoretical work.30,31 The description of the cell–substrate friction in these modeling approaches can be linked to our controlled variation of ligand affinity. Hence, our work underpins the idea that friction phenomena at the cell–substrate interface are essential for a detailed description of mechanosensitive cell adhesion.
Polyacrylamide hydrogels with defined elasticity were prepared from stock solutions of 30% acrylamide and 2% N,N′-methylenebisacrylamide (Carl Roth, Karlsruhe, Germany) in varying ratios, 0.8 wt% tetramethylethylenediamine (AppliChem GmbH), 0.5 wt% ammonium persulfate (Merck) and 0.5 μm green-fluorescent microspheres (Molecular Probes, Life Technologies, Darmstadt, Germany) were embedded. The solution was pipetted on a non-wetting coverslip (coated with Sigmacote, Sigma Aldrich, St. Louis, MO, USA) and subsequently covered by the coverslip. After 20 min polymerization the silanized coverslip with the hydrogel was gently lifted, washed in ultrapure water for 30 min and dried in a vacuum oven (Memmert, Schwabach, Germany) at room temperature and 5 bar for 45 min.
For the preparation of substrate surfaces with a tuned affinity for adhesion ligands, the dried hydrogel layers were spin-coated (Spin 150, SPS Europe B.V., TS Putten, Netherlands) with a solution of maleic anhydride copolymers. Solutions of 0.14 wt% poly(styrene-alt-maleic anhydride) (PSMA, MW = 30000 g mol−1) in tetrahydrofuran (p.a., AppliChem GmbH) or 0.3 wt% poly(ethene-alt-maleic anhydride) (PEMA, MW = 125000 g mol−1) in 1:2 acetone (p.a., AppliChem GmbH) and tetrahydrofuran were used for the spin-coating process. The monomolecular maleic anhydride copolymer film (dry thickness: a few nm)47,48 is attached to the surface of the polyacrylamide hydrogel providing a modulated affinity of adsorbed fibronectin ligands due to the hydrophobicity and polarity of the maleic anhydride copolymer surface13,49,50 (an in-depth chemical analysis of the covalent coupling scheme of the maleic anhydride copolymers to polyacrylamide hydrogels will be published in a forthcoming publication). As the monomolecular polymer layer swells under aqueous conditions the mechanical properties of the bulk hydrogel substrate are not altered.13,48 Finally, coverslips were fixed in punched polystyrene Petri dishes and washed three times in phosphate buffered saline (PBS, Biochrom, Berlin, Germany) to remove non-bound polymers and stored in PBS overnight at 4 °C. Young's modulus of hydrogel layers was determined by scanning force spectroscopy (Nanowizard3, JPK Instruments, Berlin, Germany), ranging from 2.5 kPa to 9 kPa.
Total traction force Ftot was calculated by summing up the magnitude of all traction stress vectors within the cell border multiplied by cell area. The net contractile moment Mnet was determined as the trace of the first force moment matrix . The strain energy U was calculated by and denotes the energy stored in the hydrogel deformation. Tmax was determined as the maximum traction stress within one traction stress field.
Other analyses were performed with non-smoothed force curves. In regime 1 a linear fit was applied to the time interval containing force values whose magnitude was between 15% and 80% of the local maximum. For the time interval of regime 2 (between the transition time and the end of measurement after 2 h) the geometric mean of force values was calculated, because the force values in regime 2 follow a log-normal distribution. These values were termed plateau values. Averaged values derived from different curves are shown as arithmetic mean ± standard error unless noted otherwise. Statements of statistical significance were evaluated by means of a multi-way ANOVA test with p < 0.05.
Fig. 1 Scheme of substrate design with a polyacrylamide hydrogel layer of varying crosslinking degree and elasticity as well as a surface coating with maleic anhydride copolymers, allowing for the adsorption of adhesion ligands (fibronectin) with varying affinity due to variation in polarity and hydrophobicity of the polymer coating.56 |
The time course of spreading is in accordance with the spreading phases introduced by Dubin-Thaler et al.23 The lag phase corresponds to P(hase)0, fast spreading is related to P1 and P2 is entered as spreading slows down and the maximum area is reached. Referring to the substrate property dependence our findings are somewhat contradictory to studies that state a stiffness dependent cell area for fully spread cells.5,11,44 The weak increase for stiffer substrates found in our work, which did not prove to be statistically significant, might be related to the fact that this behavior depends on the investigated cell type and the range of substrate stiffness. Weng et al.43 reported a severe stiffness sensitivity of HUVECs on PDMS micropost arrays, whose effective stiffness range is in a comparable range to that of our substrates. The reported spread areas at 10 kPa are of the same magnitude (3000 μm2) as in our experiments, but a dramatic decrease of spread area on soft substrates (at around 1 kPa) was reported in the cited study. The negligible effect observed in our experiments may be accounted for the different substrate properties (limited adhesive area on microposts, independent deformation of microposts) or variations in cell culture conditions (cell culture medium). The observation that ligand affinity has no impact on cell area agrees with previous findings: one can assume that the high ligand density used herein enables the cells to reach a fully spread state, because of the high availability of ligands for cell adhesion, masking effects of the substrate affinity on spreading.13 The trend of the characteristic time τ is interesting in the context of recent modeling efforts,29,31 which indicated a similar trend of faster spreading on stiffer substrates. Furthermore, the nonlinear model introduced therein31 suggests a smaller slope for substrates with a lower cell–substrate friction. The friction coefficient of the model was assumed to depend on substrate stiffness as well as on binding/unbinding events and density of ligand–receptors pairs. A lowering of ligand affinity to the underlying substrate, as in our setup, can be interpreted as an increase of the unbinding rate constant in the model leading to a weaker dependence of the friction coefficient on substrate stiffness. This model prediction nicely fits our experimental observations.
The spreading of cells is closely linked to the generation of traction forces. Therefore, we compared the time course of total force Ftot with the development of cell area during cell adhesion as shown for a typical example in Fig. 3A and B (see also Fig. S2, ESI†). After a short, initial phase of very weak forces, a phase of fast, nearly linear increase of Ftot was observed, saturating at later stages. The phase of fast increase of Ftot was delayed relative to the phase of fast increase in cell area by 10 min in the example shown, while average retardation time from all experiments was around 25 min. Hence, the time course of traction force evolution can be subdivided into two distinct regimes. During the very first phase, cells do not exert considerable forces, but start to quickly increase spread area. We refer to this phase as ‘regime 0’, because we focus on regimes with considerable traction forces in our analysis. Regime 0 is followed by a regime with a fast and linear increase in traction force correlated with a further small increase in area. This phase is referred to as ‘regime 1’ in the following (see Fig. 3C). As traction forces and cell area saturate later on, ‘regime 2’ is entered. In regime 2 traction forces do not exceed a certain force level, which is known to be influenced by the cell type's specific contractility and whose magnitude is given by substrate characteristics (see next section). After traction force saturation, fluctuations and relaxation of traction forces were sometimes observed, which were also reported in the literature.19,54 These phenomena were not examined herein.
Little is known about the relationship between spreading and traction force evolution in early cell adhesion. Reinhart-King et al. reported a linear correlation of total cell force and cell area during spreading even at times when actin stress fibers had not yet been assembled.28 Other measurements using cantilever based force sensors showed that the fast increase of contractile forces coincides with the formation of small paxillin stained adhesion sites.33 These reports are in line with our findings. We always observed a time lag between area and traction force increase. Recent experiments and modeling approaches further support these results.30,31
At late time points (regime 2) the traction force increase was low, forces saturated or even decreased. The latter events are often caused by a change in cell behavior. For example, the cell locally retracts its cell edge or reorients its axis, which is accompanied by the assembly and disassembly of adhesion sites. The actin cytoskeleton might account for this drop in cell traction forces. It is known that the adaptation of the contractile actin cytoskeleton in response to external forces leads to a force relaxation,54 too. Fluctuations in forces have also been reported for cells that had enough time to settle and equilibrate their forces.19 In the following, the forces in regime 2 will be treated as fluctuating around a mean value, which is given by the cell's contractility and substrate characteristics, and which describes the force homeostasis of the cell.
From a brief look a dependence of the slope of Ftot(t) in regime 1 on substrate elasticity was apparent, see Fig. 4A. By a linear fit within the time frame of regime 1, we found a higher rate of traction force increase for stiffer gels, depicted in Fig. 4B. In addition, a slight but constant offset to higher rates of force increase was found for the polymer coating with higher fibronectin affinity (PSMA) at each elasticity. These higher rates correlate with smaller transition times tR1–R2 between regime 1 and regime 2 (Fig. 4C), supporting the above statements. Hence, on stiff hydrogels (9 kPa) the transition to regime 2 occurred at about 35 min, whereas on soft hydrogels (2 kPa) it took about 50 min until traction force saturated. Both effects of faster increase and earlier saturation of Ftot did not completely compensate. Thus, the plateau values of Ftot in regime 2 were not equal for all conditions (Fig. 4D). The plateau values of Ftot increased with the hydrogels' Young's modulus in a nonlinear manner with a weaker increase for higher stiffness. Furthermore, higher ligand affinity (PSMA) resulted in a constant offset to higher plateau values of Ftot.
The same trends (as for Ftot, i.e. faster saturation and higher plateau values) were observed for the first moment of contractile force, the net contractile moment Mnet, which was evaluated, too (data not shown). For the calculation of Mnet the centripetal part of traction forces is weighted by the distance to the cell center, thus cell polarization would be manifested in Mnet. As mentioned earlier, the cells held an almost circular morphology over the observed time period without significant occurrence of polarization and elongation. In addition, the localization of traction forces at cell borders was inherent to cells on all substrates. As a result Ftot and Mnet have similar dynamics during early cell adhesion.
Finally, we had a look on two other indicators of traction forces in regime 2, the maximum traction stress Tmax and strain energy U. While Tmax is in general more noisy due to its restriction to a local point, we previously suggested it as a sensitive measure of force regulation on the length scale of receptors and adhesion sites.13 In our current study, we found a sharp increase of Tmax from 2.5 kPa to 5 kPa but no further increase for stiffer substrates (see Fig. 5A). Thus the saturation of the traction force, which was found for Ftot at high stiffness (Fig. 4D), is more apparent for Tmax with no further increase above the value at 5 kPa. This finding can be related to the difference in the local and global characteristics of Tmax and Ftot, respectively. The cells reach their maximum traction force at single adhesion sites already around a substrate stiffness of 5 kPa, however, an increase of integrated global traction forces can occur by the formation of additional traction force centers distributed over the cell area. The difference in Tmax between the substrates with different affinities is not as pronounced as for the total force Ftot, but again a constant offset to higher traction stress was observed for a higher ligand affinity (PSMA).
Another trend was found for the strain energy U, the energy stored in the gel by the adherent cell (Fig. 5B). A maximum of U was observed for medium stiffness, which can be related to the observed stiffness dependence of Ftot. The increase in strain energy from soft to medium stiffness correlates with the sharp increase in Ftot. At higher stiffness almost no additional increase in traction forces was observed, which results in the observed decrease in U as strain at constant force decreases with increasing stiffness, recall . For the lower stiffness range the strong force increase dominates the impact on U. This leads to the observed behavior of U with a maximum at an intermediate Young's modulus of 5 kPa.
In agreement with other recent studies31 traction forces are not only higher on stiffer substrates after cells reached a steady state but higher force magnitudes are already apparent at traction force increase during cell spreading. This is interesting, because focal adhesions and stress fibers, as some cellular structures known to be stiffness sensitive, have not yet been assembled to fully functional units at this stage.
The impact of ligand affinity was apparent in all regimes of considerable force generation, implying its direct impact on regulatory cell components. More precisely, increasing ligand affinity caused an increase of traction force (Fig. 4D). This behavior is superimposed onto the elasticity dependence. The higher traction force at higher ligand affinity was already apparent at the early stage of traction force evolution with higher slopes in the total force increase (Fig. 4B).
The affinity between adsorbed ligands and the underlying substrate is known to influence the force balance of cells and thus the formation of adhesion sites.13,14 In this earlier work we demonstrated a direct correlation of modulated ligand–substrate affinity and traction force magnitude, see also the short summary in the beginning of the results section. Additionally, the mobility of adhesion ligands under external forces is known to affect the assembly of mechanosensitive adhesion sites.15
From the above findings and statements we conclude that part of the cell's contractile work is dissipated in the ligand layer due to the substrate–ligand friction. This energy dissipation depends on the ligand affinity and the resulting molecular ligand friction on the underlying polymer. Only a fraction of cellular contractile work is stored as substrate deformation in the underlying hydrogel via the integrin–fibronectin link. Both processes, the elastic hydrogel deformation and the viscous ligand friction, contribute independently to substrate's mechanical properties as the process of hydrogel deformation can be treated as linearly elastic on the time scale of the dissipative friction process (some seconds). One can roughly estimate the dissipated power of the friction process taking Ftot (≈103 nN) and the ligand frictional drag velocity vd (≈10−1 μm s−1).14 An upper estimation of the dissipated power of approx. 10−1 pJ s−1 and the reasonable assumption of a seconds time scale of the traction force generation (e.g. life time of integrin–fibronectin bond) suggest a considerable influence of this viscous contribution on cell behavior when compared with the elastic deformation energy of the substrate U (≈0.5 pJ). This estimation correlates with our findings that an impact of ligand affinity could be observed in the experiments on traction force evolution. Furthermore, this mechanism should already act at early time periods of force evolution as characteristic differences are already found there. Therefore, it can be concluded that matured focal adhesions are not required for traction force generation and affinity-dependent ligand friction occurs on the molecular level of small clusters or single ligand–receptor pairs.
As there are only a few publications available considering the cell–substrate friction as a relevant parameter in cell adhesion, we have to discuss our findings in the light of two recent publications, which deal with the impact of the cell–substrate friction on cell spreading, adhesion and migration. Bergert et al.46 illustrated that the membrane–substrate friction can control cell migration under fluid drag. Their experiments and quantitative modeling showed that a cell–substrate friction coefficient in the order of 104 Pa s m−1 can regulate this process. This value together with a cell area in the order of 103 μm2 corresponds well with an affinity controlled ligand mobility of 105 m N−1 s−1 in our setup as earlier derived by Pompe et al.14
Another model introduced by Nisenholz et al.31 allows us to directly discuss the impact of the cell–substrate friction on the traction force evolution. Although the substrate–ligand friction was not explicitly introduced in the model, the cell–substrate friction is described in terms of binding/unbinding events on the receptor–ligand level, see also the discussion in the first part of the results section. It can be reasonably assumed that a molecular sliding friction of the ligand on the substrate, as introduced by Pompe et al.,14 can be handled in the same framework. An increase of the substrate–ligand friction, like the change from low affinity substrates (PEMA) to high affinity substrates (PSMA), can be described as an effective decrease of the unbinding rate constant in the model of Nisenholz et al., leading to an increase of the effective interfacial friction coefficient ξs. It is very interesting to note that with this assumption the nonlinear model nicely captures our experimental findings of an increase of Ftot, and a steeper negative slope of τ(E) (Fig. 2C) at a higher substrate–ligand affinity. Hence, we suggest both models as good starting points for an explicit description of the substrate–ligand friction.
In summary, our study proves that the cell–substrate friction has a considerable influence on the adaption of cells to their surroundings. It demonstrates viscoelasticity of the extracellular environment not only to affect the magnitude of traction forces but also determine the dynamics of force evolution in an additive way, already at early time periods of cell spreading without a fully established focal adhesion and stress fiber apparatus. We expect our experimental findings to stimulate further progress in the description of the dynamic cell behavior in viscoelastic environments.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/c5sm01706h |