Phosphorus-doped NiCo2S4 nanocrystals grown on electrospun carbon nanofibers as ultra-efficient electrocatalysts for the hydrogen evolution reaction

Huahao Gu a, Wei Fan *b and Tianxi Liu *ab
aState Key Laboratory of Molecular Engineering of Polymers, Department of Macromolecular Science, Fudan University, 220 Handan Road, Shanghai 200433, P. R. China. E-mail: txliu@fudan.edu.cn; txliu@dhu.edu.cn; Fax: +86-21-65640293; Tel: +86-21-55664197
bState Key Laboratory for Modification of Chemical Fibers and Polymer Materials, College of Materials Science and Engineering, Donghua University, 2999 North Renmin Road, Shanghai 201620, P. R. China. E-mail: weifan@dhu.edu.cn

Received 7th May 2017 , Accepted 15th June 2017

First published on 15th June 2017


Abstract

The development of highly efficient noble-metal-free electrocatalysts for the hydrogen evolution reaction (HER) is still a challenge nowadays. In this work, we prepared a highly active electrocatalyst containing phosphorus-doped NiCo2S4 nanocrystals grown on carbon nanotube embedded carbon nanofibers (P-NiCo2S4@CNT/CNF). The CNTs are involved in enhancing the electrical conductivity of the three-dimensional CNF network through a facile co-electrospinning method, which can facilitate electron transfer to the attached HER active material. Templated by this nanofiber network, the electroactive NiCo2S4 is confined to grow perpendicularly onto the CNT/CNF template via a hydrothermal reaction, thus exposing more catalytic active sites. Doping of P into the hybrid via a phosphidation reaction improves the electronic structure of the electroactive NiCo2S4, thus decreasing the energy barrier during the HER process. Owing to the synergistic effects from electrical enhancement and the nanostructured morphology, along with P-doping-induced optimization of the electronic structure, the P-NiCo2S4@CNT/CNF hybrid exhibits excellent HER performance, with an ultra-low onset overpotential (η) of 27 mV, a remarkable current density of 10 mA cm−2 at η as low as 74 mV, an impressive exchange current density of 0.79 mA cm−2 and excellent long-term durability. Furthermore, its electroactivity exceeds that of most reported noble-metal-free electrocatalysts and is comparable to that of Pt, suggesting its great potential as a highly efficient HER catalyst.



Conceptual insights

Nickel cobalt sulfide (NiCo2S4), a ternary transition metal sulfide, has been largely reported as an electrode material in supercapacitors and lithium batteries. However, there is little detailed research on its application as an electrocatalyst for the hydrogen evolution reaction (HER). In this communication, NiCo2S4 is introduced as the HER active material grown on a template of carbon nanofibers, thus fully exposing its electrocatalytic sites. Despite its nanoscale structure, the hybrid exhibits an average performance in electrocatalysis. In this case, phosphorus (P) is delicately designed to dope into the electrocatalytically active NiCo2S4, which can modify the inherent electronic structure of catalysts, thus reducing the kinetic energy barrier in the HER process, and greatly enhancing its performance. Consequently, this communication not only broadens the application of NiCo2S4 in the energy field, but also provides an efficient method of doping to largely improve the HER activity of electrocatalyst.

1. Introduction

Hydrogen evolution through electrolysis of water provides a promising method to store energy from renewable sources.1,2 Highly efficient electrocatalysts are required to promote the sluggish kinetics of the hydrogen evolution reaction (HER). Noble metals such as Pt are the state-of-the-art HER catalysts, but their scarcity and high cost limit their global-scale applicability. Recently, researchers have been developing high-performance earth-abundant metal chalcogenides, carbides, nitrides, or phosphides to replace Pt as electrocatalysts.3–6 However, to the best of our knowledge, the existing reports mainly focus on researching some binary metal compounds, such as CoS2, MoSe2, Mo2C and Ni2P, while only a few HER catalysts comprising ternary metal compounds have been reported. Nickel cobalt sulfide (NiCo2S4), a ternary transition metal sulfide, is intrinsically a conductive metal, which possesses an extremely high electrical conductivity7 (∼100 times as high as that of NiCo2O4, and much higher than those of the binary cobalt sulfides and nickel sulfides).8,9 It has been reported that NixCo3−xS4 polyhedra synthesized by transforming metal–organic frameworks through solvothermal sulfidation exhibit excellent HER activities, indicating the great potential of NiCo2S4 as an efficient electrocatalyst for hydrogen generation.10

In order to further improve the HER energy conversion efficiency, a general method is to hybridize the electroactive material with a highly conductive template to make a hybrid product. It is well known that the catalytic activity of an electrocatalyst is greatly influenced by the density of active sites. Hence, by introducing a conductive template with a large surface area, the electroactive material is confined to grow into a nanoscale structure, thus maximizing the exposure of HER active sites, as well as guaranteeing the fast electron transport in the hybrid. Carbon nanofiber (CNF) membranes with a three-dimensional (3D) network structure, high surface-to-volume ratio, and good conductivity have been commonly used as conductive templates in electrochemical energy storage and conversion devices.11 Electrospinning techniques offer a versatile way to construct 3D CNF networks and their hybrids with tunable structures.12,13 The performance of the electrospun nanofibers can be easily adjusted by changing the components of the spinning solution. For example, NiCo2O4-doped CNF membranes can be formed through co-electrospinning of polyacrylonitrile (PAN) and nickel–cobalt layered double hydroxide (Ni–Co LDH), followed by carbonization.14 The uniformly distributed NiCo2O4 nanoparticles in CNF increase the conductivity of CNF and enhance the pseudocapacitive performance for supercapacitor applications.

Apart from constructing hierarchical hybrids of confined electroactive material with a highly conductive template, doping of non-metal heteroatoms into electrocatalysts is an effective approach to intrinsically improve the HER activity. The enhanced HER activities are contributed by the improved charge transfer between the foreign atom and the host atom, along with the modified inherent electronic structure reducing the kinetic energy barrier during the hydrogen generation pathway.15 Gong et al. prepared ultrathin MoS2(1−x)Se2x alloy nanoflakes with monolayered or few-layered thickness, which exhibited enhanced electrocatalytic performance in comparison with either MoS2 or MoSe2. The improvements resulted from the higher intrinsic activity of doped catalysts with tuned hydrogen adsorption free energy (ΔGH) closer to thermoneutral.16 A similar result has also been reported for WS2(1−x)Se2x nanotubes.17 Despite doping or alloying with non-metal elements from the same group, more remarkable adjustment of electronic structure is expected to occur in the case of doping with non-metal heteroatoms from different groups, such as doping selenium to phosphor, and chlorine to sulfur. For example, a selenium-doped pyrite-phase NiP2 nanostructure was designed for HER catalysis, and a current density of 10 mA cm−2 was achieved at an overpotential as low as 84 mV, which was far smaller than that of pure NiP2 (135 mV), highlighting the significant effect induced from doping or alloying electrocatalysts with non-metal element from another group.18

Herein, P-doped NiCo2S4 grown on carbon nanotube reinforced carbon nanofibers (P-NiCo2S4@CNT/CNF) has been prepared as a hybrid catalyst for the HER. CNTs are embedded into the CNF membrane via a facile co-electrospinning process, which is designed to increase the electrical conductivity of the template, facilitating the charge transfer between the CNT/CNF template and electroactive NiCo2S4 nanocrystals. P, a non-chalcogen heteroatom, is doped into NiCo2S4 to tune the electronic structure, thus optimizing the hydrogen adsorption energy of the hybrid catalyst. As a consequence, the P-NiCo2S4@CNT/CNF hybrid exhibits superb HER activity, with a large cathodic current of 10 mA cm−2 at a low overpotential of 74 mV, an impressive exchange current density of 0.79 mA cm−2, suggesting the rational design of the electrocatalyst.

2. Experimental

2.1. Preparation of P-NiCo2S4@CNT/CNF membranes

CNT/CNF membranes were prepared via facile co-electrospinning of polyacrylonitrile (PAN) and CNT dispersions, followed by pre-oxidation and carbonization (see the ESI for experimental details). NiCo2S4@CNT/CNF membranes were prepared through a one-step hydrothermal procedure. Briefly, Ni(NO3)2·6H2O (1 mmol), Co(NO3)2·6H2O (2 mmol), thiourea (8 mmol) and urea (4 mmol) were dissolved in 30 mL DI water under vigorous magnetic stirring for 20 min. After that, the transparent pink solution was transferred into a 50 mL Teflon-lined stainless steel autoclave with a piece of CNT/CNF membrane (2 × 2 cm2) immersed into the reaction solution and maintained at 160 °C for 12 h.

P-doped NiCo2S4@CNT/CNF membranes were synthesized through a phosphidation reaction in a tube furnace. The phosphidation reaction was performed at 300 °C for 1 h with a heating rate of 2 °C min−1 under a steady flow of N2 gas. After cooling down naturally, the phosphorus-doped hybrid product was prepared, and denoted as P-NiCo2S4@CNT/CNF. The whole preparation process is schematically shown in Scheme 1. For comparison, a NiCo2S4@CNT/CNF hybrid was synthesized by the same process in the absence of phosphidation reaction while a P-NiCo2S4@CNF hybrid was synthesized without the addition of CNTs during the electrospinning step. Pure NiCo2S4 was prepared by a similar process without the CNT/CNF template and the phosphidation reaction.


image file: c7nh00066a-s1.tif
Scheme 1 Schematic illustration of the preparation of the P-NiCo2S4@CNT/CNF hybrid.

2.2. Electrochemical measurements

The electrochemical measurements were carried out in a three-electrode setup using a CHI 660D electrochemical workstation (Shanghai Chenhua Instrument Co., China), with a graphite rod used as the counter electrode, a saturated calomel electrode (SCE) as the reference electrode, and the electrocatalyst modified glassy carbon electrode (GCE) as the working electrode. A piece of pre-cut hybrid membrane was affixed onto a GCE tip by Nafion solution, with a loading amount of 0.7–0.9 mg in a 3 × 3 mm2 sized square shape. Commercial platinum wire (Pt) was also measured to establish a reference point of a state-of-the-art HER catalyst. Linear sweep voltammetry (LSV) was measured at a scan rate of 2 mV s−1 in 0.5 M H2SO4 solution. All of the potentials were calibrated to the reversible hydrogen electrode (RHE) by adding a value of (0.241 + 0.059 × pH) V. The polarization curves were replotted as overpotential (η) versus log[thin space (1/6-em)]current density (log[thin space (1/6-em)]j) to get the Tafel plots for assessing the HER kinetics. By fitting the linear portions of Tafel plots to the Tafel equation (η = b[thin space (1/6-em)]log[thin space (1/6-em)](j) + a), the Tafel slope (b) can be calculated. To determine the double-layer capacitance (Cdl) of electrocatalysts, cyclic voltammogram cycles were recorded in the region of 0.15–0.25 V vs. RHE at various scan rates. By plotting the Δj at 0.2 V vs. RHE against each scan rate, these data could be fitted to a line, whose slope is twice the geometric Cdl. Electrochemical impedance spectroscopy (EIS) measurement was performed in the same configuration under various overpotentials in frequencies ranging from 106 Hz to 10−2 Hz with an amplitude of 5 mV. The electrocatalytic stability of the catalyst was evaluated by testing current–time responses under a fixed overpotential for a period of time.

3. Results and discussion

3.1. Morphology and structure of the P-NiCo2S4@CNT/CNF hybrid

A CNT-embedded CNF membrane was fabricated through co-electrospinning, pre-oxidation, and carbonization processes. As shown in Fig. 1, the surface of CNT/CNF becomes coarse due to the incorporation of CNTs. Some CNTs are partially exposed on the surface of the CNF while major parts are embedded into the nanofibers, which can be proved by the TEM observations (Fig. 1D). Moreover, the electrical conductivity of the CNT/CNF membrane is 1.90 S cm−1, which is nearly three times that of the pure CNF membrane (Table S1, ESI), thus promoting the charge transfer between the conductive template and electroactive NiCo2S4 during the HER process.
image file: c7nh00066a-f1.tif
Fig. 1 FESEM (left) and TEM (right) images of (A and B) pristine CNF, and (C and D) CNT/CNF.

Based on the CNT/CNF template, P-NiCo2S4@CNT/CNF hybrids were prepared through a one-step hydrothermal method, followed by the phosphidation reaction. Fig. 2 shows the morphology of the NiCo2S4@CNT/CNF hybrid and P-NiCo2S4@CNT/CNF hybrid. It can be observed that NiCo2S4 nanocrystals with lengths around 200 nm are uniformly and densely grown onto the CNT/CNF template (Fig. 2A and B), whose morphology is the same as that of the NiCo2S4@CNF hybrid in general (Fig. S1, ESI). For comparison, NiCo2S4 prepared in the absence of CNT/CNF membranes forms agglomerates with inhomogeneous nanorod and nanoflake interlaced morphology (Fig. S2, ESI). Therefore, constructing hierarchical nanostructures of NiCo2S4 nanocrystals perpendicularly grown onto CNT/CNF can greatly prevent the aggregation of NiCo2S4, effectively exposing the electrocatalytic sites. After the phosphidation reaction, the overall morphology of the obtained P-NiCo2S4@CNT/CNF hybrid remains almost the same as that of NiCo2S4@CNT/CNF (Fig. 2C and D). However, EDS mapping clearly reveals the existence of P element in the P-NiCo2S4@CNT/CNF hybrid in addition to Ni, Co, C, and S elements (Fig. 2H). Compared with the EDS spectra of NiCo2S4@CNT/CNF (Fig. 2J and Fig. S3F, ESI), an additional peak located at 2.01 keV can be found for the P-NiCo2S4@CNT/CNF hybrid, which refers to pKa energy, confirming the successful doping of P element via phosphidation reaction.19


image file: c7nh00066a-f2.tif
Fig. 2 FESEM images of (A and B) the NiCo2S4@CNT/CNF hybrid and (C and D) the P-NiCo2S4@CNT/CNF hybrid, (E–I) EDS mapping images of the P-NiCo2S4@CNT/CNF hybrid, and (J) EDS spectrum of the P-NiCo2S4@CNT/CNF hybrid.

The phase purity of the as-prepared products has been investigated by XRD analysis (Fig. 3A). The CNT/CNF membrane shows a broad and weak peak at 2θ = 26°, implying its amorphous structure. The XRD pattern of the NiCo2S4@CNT/CNF hybrid displays diffraction peaks at 2θ = 16.7°, 27.2°, 31.9°, 38.6°, 50.8° and 55.6°, which can be, respectively, attributed to the (111), (220), (311), (400), (511), and (440) planes of NiCo2S4 (JCPDS 20-0782).20,21 The XRD pattern of the P-NiCo2S4@CNT/CNF hybrid is consistent with that of the NiCo2S4@CNT/CNF hybrid, illustrating that the incorporation of P element does not cause changes in the XRD pattern of the hybrid, and a similar phenomenon has been reported previously.22 In addition, for the synthesized NiCo2S4 agglomerates in the absence of CNT/CNF template, although its main diffraction peaks can be attributed to the planes of NiCo2S4, there appear several small extra peaks with impurities, suggesting that the attached NiCo2S4 nanocrystals can grow in higher purity with the support of the 3D CNT/CNF template.


image file: c7nh00066a-f3.tif
Fig. 3 (A) XRD patterns of different products. (B) Raman spectra of the NiCo2S4@CNT/CNF and P-NiCo2S4@CNT/CNF hybrids. (C–F) XPS spectra of the NiCo2S4@CNT/CNF and P-NiCo2S4@CNT/CNF hybrids: high-resolution (C) Co 2p, (D) Ni 2p, (E) S 2p, and (F) P 2p spectra.

Further insights into the structural changes after doping of P element could be acquired from the Raman spectra and XPS analysis. As shown by the Raman spectra in Fig. 3B, the NiCo2S4@CNT/CNF hybrid displays four peaks at 241.7 cm−1, 384.9 cm−1, 305.7 cm−1, and 352.9 cm−1, which are the characteristic Eg, A1g, and two T2g vibration modes of NiCo2S4.7 Besides, some additional vibration modes in the range of 400 cm−1–800 cm−1 can be obviously observed, which can be well indexed to the Raman features of NiCo2O4,23 as the surface of transitional metal sulfides can be easily oxidized once exposed to air.24,25 After the phosphidation reaction, the peaks in the range of 400 cm−1–800 cm−1 disappeared for the P-NiCo2S4@CNT/CNF hybrid, which is due to the fact that the released PH3 during phosphidation can reduce the superficial oxide impurities into the P-doped NiCo2S4 hybrid.

As shown in Fig. 3C, the Co 2p spectrum displays low energy bands (Co 2p3/2) and high energy bands (Co 2p1/2).26 Specifically, the binding energies centered at 779.40 eV and 794.60 eV of the Co 2p peaks correspond to the Co3+ state while those at 783.70 eV and 799.20 eV are characteristic of the Co2+ state. Similarly, for the Ni 2p spectrum, the peaks located at 854.20 eV and 871.50 eV can be respectively assigned to Ni 2p3/2 and Ni 2p1/2 spin orbits of the Ni2+ state, and those situated at 857.90 eV and 876.20 eV are associated with the Ni3+ state.21,27 Besides, it is interesting to notice that the relative peak intensities of the Ni2+ state and Co3+ state for the P-NiCo2S4@CNT/CNF hybrid are higher than those for the NiCo2S4@CNT/CNF hybrid, further confirming that NiCo2S4 in the P-NiCo2S4@CNT/CNF hybrid shows much higher crystalline purity. For the S 2p spectrum, the S 2p spectrum has been fitted with spin–orbit doublet separation of 1.18 eV and an area ratio of 2[thin space (1/6-em)]:[thin space (1/6-em)]1. The peaks located at 161.00 eV and 162.18 eV, respectively, correspond to S 2p3/2 and S 2p1/2 orbits of divalent sulfide ions (S2−). However, no obvious peak can be fitted for the S22− 2p3/2 and S22− 2p1/2 at 163.20 eV and 164.38 eV, indicating that no S-rich structure exists in the P-NiCo2S4@CNT/CNF and NiCo2S4@CNT/CNF hybrids. Moreover, an extra peak at 168.30 eV induced by sulfur oxide can be obviously observed for the S 2p spectrum of the NiCo2S4@CNT/CNF hybrid, which is not observed for the P-NiCo2S4@CNT/CNF hybrid. This further confirms that phosphidation reaction helps to remove some sulfur oxides triggered by surface air oxidization, which is consistent with the Raman results.28 With regard to the P 2p spectrum of the P-NiCo2S4@CNT/CNF hybrid, two peaks with binding energies of 128.90 eV and 129.90 eV are, respectively, assigned to P 2p3/2 and P 2p1/2, along with a characteristic peak attributed to phosphate-like P at 133.45 eV.19,29,30 As a result, although phosphidation reaction removes the S–O peak, it induces a P–O peak of phosphate at the same time. However, some studies report that metal phosphates are electrocatalytically active to a certain degree.31,32 By contrast, the NiCo2S4@CNT/CNF hybrid does not show any significant peaks in the corresponding range of binding energy. All the above results strongly prove the successful doping of P element into the NiCo2S4@CNT/CNF hybrid.

3.2. HER electrocatalytic activity of the P-NiCo2S4@CNT/CNF hybrid

The electrocatalytic performance of the HER catalysts was measured with a standard three-electrode setup in 0.5 M H2SO4 electrolyte. From the polarization curves in Fig. 4A, it is shown that the onset overpotential (η) is only 27 mV for the P-NiCo2S4@CNT/CNF hybrid, which is the lowest among all the as-prepared products. Moreover, the drive current density (j) of 10 mA cm−2, a characteristic value for solar fuel conversion, can be achieved at a small overpotential of 74 mV for the P-NiCo2S4@CNT/CNF hybrid, compared with 126 mV for the P-NiCo2S4@CNF hybrid, 164 mV for the NiCo2S4@CNT/CNF hybrid and 278 mV for NiCo2S4, respectively. As is well known, an excellent electrocatalyst is desirable to drive significant current densities with low overpotentials. Therefore, the P-NiCo2S4@CNT/CNF hybrid exhibits the optimal HER activities among all the prepared products, demonstrating that P doping, CNT reinforcement, and template-confined growth can help enhance the electrocatalytic performance of catalysts. Furthermore, it is worth noting that for the same current density (j = 10 mA cm−2), the difference of the required overpotential between the NiCo2S4@CNT/CNF and P-NiCo2S4@CNT/CNF electrocatalysts is up to nearly 100 mV, highlighting the significant impacts induced by P-doping. The electrochemical double-layer capacitance (Cdl), which is linearly proportional to the electrocatalytically active surface area, was investigated to explain the differences in HER performance of various catalysts. As shown in Fig. 4B and Fig. S4 (ESI), the Cdl of the P-NiCo2S4@CNT/CNF hybrid is tested to be 33.8 mF cm−2, which is far beyond that of other counterparts, indicating the existence of more electrocatalytic sites. The unique nanostructure of the P-NiCo2S4@CNT/CNF hybrid makes great contributions to its increased HER active sites. First, the electronic structure of catalytically active NiCo2S4 can be improved with P doping, thus tuning the hydrogen adsorption free energy (ΔGH) closer to thermoneutral. Second, CNTs increase the electrical conductivity of the CNF template, which facilitates the electron transport between the 3D template and NiCo2S4 nanocrystals. Last but not least, with the CNT/CNF network, NiCo2S4 is confined to grow into perpendicularly oriented nanocrystals instead of agglomerates, thus constructing a hierarchical structure with exposed active sites on a nanoscale size. These synergistic effects lead to the increase in the number of catalytic sites of the P-NiCo2S4@CNT/CNF hybrid, making contributions to its distinctive HER performance.
image file: c7nh00066a-f4.tif
Fig. 4 (A) LSV polarization curves for the CNT/CNF, NiCo2S4, and NiCo2S4@CNT/CNF and P-NiCo2S4@CNT/CNF hybrid modified GCE in N2-purged 0.5 M H2SO4 solution. (B) Plot showing the extraction of the double layer capacitance (Cdl) for the different hybrids at 0.2 V versus RHE. (C) Tafel plots for the different hybrid modified GCEs. (D) Nyquist plots of the different hybrids at overpotential of 0.17 V versus RHE.

In addition, Tafel plots are derived by plotting overpotential (η) against log[thin space (1/6-em)]current (log[thin space (1/6-em)]j), and the kinetic parameters can be calculated (Fig. 4C). The linear parts of the Tafel plots reveal that Tafel slopes of all prepared electrocatalysts are in the range of 60 mV decade−1–75 mV decade−1, suggesting that the HER activities proceed via a fast Volmer reaction, followed by a rate-limiting Heyrovsky step. The exchange current density, j0, which is obtained from the Tafel curves with the extrapolation method, can reflect the inherent HER activity of the catalyst. As shown in Fig. S5 and Table S2 (ESI), the exchange current density (j0) for the P-NiCo2S4@CNT/CNF hybrid is 0.79 mA cm−2, which is 4–20 times larger than that of the other hybrids, presenting its intrinsic outstanding activity for HER catalysis. The large j0 can be attributed to the P-doping induced change in electronic structure of NiCo2S4, which further lowers the kinetic energy barrier during the hydrogen formation process, thus generating a remarkable improvement in the inherent catalytic performance. It is worth mentioning that the HER activities of the P-NiCo2S4@CNT/CNF hybrid exceed most reported studies (Table 1), further illustrating its ultra-high catalytic ability. The electrochemical impedance spectroscopy (EIS) measurement was also explored under the HER process (Fig. 4D). Nyquist plots reveal that the P-NiCo2S4@CNT/CNF hybrid shows the smallest charge transfer resistance (Rct) of 4.7 Ω among all the products, reflecting its rapid electron transfer compared with its counterparts.

Table 1 Comparison of the HER activity of the P-NiCo2S4@CNT/CNF hybrid to the reported electrocatalysts
Sample η 0 (mV) η 10 (mV) Ref.
η 0: onset overpotential; η10: overpotential (η) for current density (j) of 10.0 mA cm−2.
Mn0.05Co0.95Se2 174 195 33
NiP1.93Se0.07/carbon paper 84 18
Co-doped MoS2/carbon black 90 135 34
Hollow Zn0.30Co2.70S4 35 80 10
MoS2/CoS2/carbon cloth 87 35
P doped MoO2 on Mo foil 80 135 19
CoxW(1−x)S2 121 36
SnS/N-doped graphene 59 125 37
P-NiCo2S4@CNT/CNF 27 74 This work


The stability of the P-NiCo2S4@CNT/CNF catalyst was measured through performing continuous HER activities at a constant overpotential of 125 mV. As shown in Fig. 5A and B, there occurs only a slight fluctuation in such a large current density (around 40 mA cm−2) for 10 h, along with no distinct changes in its polarization curves measured after cycling. Furthermore, the charge transfer resistance (Rct) only slightly increases from 7.9 Ω to 9.1 Ω (Fig. 5C) after cycling for 10 h. All the results indicate the excellent HER stability of the P-NiCo2S4@CNT/CNF hybrid catalyst, which can be attributed to its robust morphology that is retained well during the violent hydrogen evolution reaction (Fig. 5D).


image file: c7nh00066a-f5.tif
Fig. 5 (A) Time dependence of the current density for the P-NiCo2S4@CNT/CNF hybrid modified GCE recorded at −0.17 V versus RHE. (B) Comparison of LSV polarization curves for the P-NiCo2S4@CNT/CNF hybrids before and after the cycling test. (C) Comparison of Nyquist plots for the P-NiCo2S4@CNT/CNF hybrids before and after the cycling test. (D) FESEM image of the P-NiCo2S4@CNT/CNF hybrids after the cycling test.

4. Conclusions

In summary, we have successfully prepared P-NiCo2S4@CNT/CNF hybrid catalysts by combining electrospinning, a hydrothermal method, and phosphidation reaction. The involvement of CNTs increases the electrical conductivity of the CNF template, which provides fast electron transfer to the attached NiCo2S4 nanocrystals. Templated by the CNT/CNF network, NiCo2S4 is confined to grow into perpendicularly oriented nanocrystals instead of agglomerates, thus constructing a hierarchical structure with increased electrocatalytically active sites. The phosphidation reaction realizes the doping of P into the hybrid, thereby decreasing the kinetic energy barrier. Consequently, the P-NiCo2S4@CNT/CNF hybrid exhibits outstanding HER activities with a low onset overpotential (η) of 27 mV, a large cathodic current of 10 mA cm−2 at η of only 74 mV, an impressive exchange current density of 0.79 mA cm−2 and excellent long-term durability in acid solution, which are superior to most reported noble-metal-free electrocatalysts and comparable to that of Pt. The strategy of heteroatom doping into electroactive materials and conductivity enhancement on templates, provides an efficient method to fabricate highly active electrocatalysts for energy conversion.

Acknowledgements

The authors are grateful for the financial support from the National Natural Science Foundation of China (51433001, 51373037), and the Program of Shanghai Academic Research Leader (17XD1400100).

Notes and references

  1. A. G. Tamirat, J. Rick, A. A. Dubale, W. N. Su and B. J. Hwang, Nanoscale Horiz., 2016, 1, 243–267 RSC.
  2. A. Vasileff, S. Chen and S. Z. Qiao, Nanoscale Horiz., 2016, 1, 41–44 RSC.
  3. F. L. Lai, D. Y. Yong, X. L. Ning, B. C. Pan, Y. E. Miao and T. X. Liu, Small, 2016, 1602866 Search PubMed.
  4. W. Gao, Y. Q. Shi, Y. F. Zhang, L. Z. Zuo, H. Y. Lu, Y. P. Huang, W. Fan and T. X. Liu, ACS Sustainable Chem. Eng., 2016, 4, 6313–6321 CrossRef CAS.
  5. Y. Pan, Y. Lin, Y. J. Chen, Y. Q. Liu and C. G. Liu, J. Mater. Chem. A, 2016, 4, 4745–4754 CAS.
  6. K. Ojha, S. Saha, B. Kumar, K. S. Hazra and A. K. Ganguli, ChemCatChem, 2016, 8, 1218–1225 CrossRef CAS.
  7. C. Xia, P. Li, A. N. Gandi, U. Schwingenschlögl and H. N. Alshareef, Chem. Mater., 2015, 27, 6482–6485 CrossRef CAS.
  8. W. B. Fu, C. H. Zhao, W. H. Han, Y. Liu, H. Zhao, Y. F. Ma and E. Q. Xie, J. Mater. Chem. A, 2015, 3, 10492–10497 CAS.
  9. C. Xia and H. N. Alshareef, Chem. Mater., 2015, 27, 4661–4668 CrossRef CAS.
  10. Z. F. Huang, J. J. Song, K. Li, M. Tahir, Y. T. Wang, L. Pan, L. Wang, X. W. Zhang and J. J. Zou, J. Am. Chem. Soc., 2016, 138, 1359–1365 CrossRef CAS PubMed.
  11. S. J. Peng, L. L. Li, J. Kong Yoong Lee, L. L. Tian, M. Srinivasan, S. Adams and S. Ramakrishna, Nano Energy, 2016, 22, 361–395 CrossRef CAS.
  12. Z. X. Dong, S. J. Kennedy and Y. Q. Wu, J. Power Sources, 2011, 196, 4886–4904 CrossRef CAS.
  13. Z. Y. Xiong, X. Y. Kong, Z. X. Guo and J. Yu, Chin. J. Polym. Sci., 2015, 33, 1234–1244 CrossRef CAS.
  14. F. L. Lai, Y. E. Miao, Y. P. Huang, T. S. Chung and T. X. Liu, J. Phys. Chem. C, 2015, 119, 13442–13450 CAS.
  15. J. K. Nørskov, T. Bligaard, A. Logadottir, J. R. Kitchin, J. G. Chen, S. Pandelov and U. Stimming, J. Electrochem. Soc., 2005, 152, J23–J26 CrossRef.
  16. Q. F. Gong, L. Cheng, C. H. Liu, M. Zhang, Q. L. Feng, H. L. Ye, M. Zeng, L. M. Xie, Z. Liu and Y. G. Li, ACS Catal., 2015, 5, 2213–2219 CrossRef CAS.
  17. K. Xu, F. M. Wang, Z. X. Wang, X. Y. Zhan, Q. S. Wang, Z. Z. Cheng, M. Safdar and J. He, ACS Nano, 2014, 8, 8468–8476 CrossRef CAS PubMed.
  18. J. Q. Zhuo, M. Cabán-Acevedo, H. F. Liang, L. Samad, Q. Ding, Y. P. Fu, M. X. Li and S. Jin, ACS Catal., 2015, 5, 6355–6361 CrossRef CAS.
  19. X. Xie, R. J. Yu, N. Xue, A. B. Yousaf, H. Du, K. Liang, N. Jiang and A. W. Xu, J. Mater. Chem. A, 2016, 4, 1647–1652 CAS.
  20. J. Yang, M. Z. Ma, C. C. Sun, Y. F. Zhang, W. Huang and X. C. Dong, J. Mater. Chem. A, 2015, 3, 1258–1264 CAS.
  21. J. G. Wang, D. D. Jin, R. Zhou, C. Shen, K. Y. Xie and B. Q. Wei, J. Power Sources, 2016, 306, 100–106 CrossRef CAS.
  22. D. Y. Wang, M. Gong, H. L. Chou, C. J. Pan, H. A. Chen, Y. P. Wu, M. C. Lin, M. Y. Guan, J. Yang, C. W. Chen, Y. L. Wang, B. J. Hwang, C. C. Chen and H. J. Dai, J. Am. Chem. Soc., 2015, 137, 1587–1592 CrossRef CAS PubMed.
  23. C. F. Windisch Jr. and G. J. Exarhos, J. Appl. Phys., 2002, 92, 5572–5574 CrossRef.
  24. L. S. Zhang, Y. P. Huang, Y. F. Zhang, H. H. Gu, W. Fan and T. X. Liu, Adv. Mater. Interfaces, 2016, 3, 1500467 CrossRef.
  25. H. H. Gu, Y. P. Huang, L. Z. Zuo, W. Fan and T. X. Liu, Electrochim. Acta, 2016, 219, 604–613 CrossRef CAS.
  26. J. W. Xiao, L. Wan, S. H. Yang, F. Xiao and S. Wang, Nano Lett., 2014, 14, 831–838 CrossRef CAS PubMed.
  27. Z. C. Li, Y. Qu, M. G. Wang, Y. M. Hu, J. Han, L. Fan and R. Guo, Colloid Polym. Sci., 2016, 294, 1325–1332 CAS.
  28. D. L. Legrand, H. W. Nesbitt and G. M. Bancroft, Am. Mineral., 1998, 83, 1256–1265 CrossRef CAS.
  29. G. Y. Xu, B. Ding, J. Pan, J. P. Han, P. Nie, Y. Zhu, Q. Sheng and H. Dou, J. Mater. Chem. A, 2015, 3, 23268–23273 CAS.
  30. W. Liu, E. Y. Hu, H. Jiang, Y. J. Xiang, Z. Weng, M. Li, Q. Fan, X. Q. Yu, E. I. Altman and H. L. Wang, Nat. Commun., 2016, 7, 10771 CrossRef CAS PubMed.
  31. J. H. Xing, H. Li, M. C. C. Mark, S. M. Geyer and K. Y. S. Ng, J. Mater. Chem. A, 2016, 4, 13866–13873 CAS.
  32. Z. X. Cai, W. Xu, F. M. Li, Q. H. Yao and X. Chen, ACS Sustainable Chem. Eng., 2017, 5, 571–579 CrossRef CAS.
  33. Y. W. Liu, X. M. Hua, C. Xiao, T. F. Zhou, P. C. Huang, Z. P. Guo, B. C. Pan and Y. Xie, J. Am. Chem. Soc., 2016, 138, 5087–5092 CrossRef CAS PubMed.
  34. X. P. Dai, K. L. Du, Z. Z. Li, M. Z. Liu, Y. D. Ma, H. Sun, X. Zhang and Y. Yang, ACS Appl. Mater. Interfaces, 2015, 7, 27242–27253 CAS.
  35. J. L. Huang, D. M. Hou, Y. C. Zhou, W. J. Zhou, G. Q. Li, Z. H. Tang, L. G. Li and S. W. Chen, J. Mater. Chem. A, 2015, 3, 22886–22891 CAS.
  36. T. A. Shifa, F. M. Wang, K. L. Liu, K. Xu, Z. X. Wang, X. Y. Zhan, C. Jiang and J. He, Small, 2016, 12, 3802–3809 CrossRef CAS PubMed.
  37. S. S. Shinde, A. Sami, D. Kim and J. Lee, Chem. Commun., 2015, 51, 15716–15719 RSC.

Footnote

Electronic supplementary information (ESI) available. See DOI: 10.1039/c7nh00066a

This journal is © The Royal Society of Chemistry 2017
Click here to see how this site uses Cookies. View our privacy policy here.