Akhil
Gupta
*a,
Anushri
Rananaware
b,
Pedada
Srinivasa Rao
cd,
Duong
Duc La
b,
Ante
Bilic
e,
Wanchun
Xiang
f,
Jingliang
Li
a,
Richard A.
Evans
g,
Sidhanath V.
Bhosale
c and
Sheshanath V.
Bhosale
*b
aInstitute for Frontier Materials, Deakin University, Waurn Ponds, Victoria 3216, Australia. E-mail: akhil.gupta@deakin.edu.au; Tel: +61 3 5247 9542
bSchool of Science, RMIT University, GPO Box 2476, Melbourne, Victoria 3001, Australia. E-mail: sheshanath.bhosale@rmit.edu.au; Tel: +61 3 9925 2680
cPolymers and Functional Materials Division, CSIR-Indian Institute of Chemical Technology, Hyderabad 500007, Telangana, India
dAcademy of Scientific and Innovative Research (AcSIR), CSIR-IICT, Hyderabad 500007, Telangana, India
eData61 CSIRO, Molecular and Materials Modelling, Docklands, Victoria 8012, Australia
fState Key Laboratory of Silicate Materials for Architectures, Wuhan University of Technology, 122 Luoshi Rd, Wuhan 430070, Hubei, P. R. China
gCSIRO Manufacturing, Bayview Avenue, Clayton South, Victoria 3169, Australia
First published on 6th April 2017
A bifluorenylidene-functionalized, H-shaped, small molecular non-fullerene electron acceptor, 6,6′,6′′,6′′′-([9,9′-bifluorenylidene]-2,2′,7,7′-tetrayltetrakis(thiophene-5,2-diyl))tetrakis(2,5-bis(2-ethylhexyl)-3-(thiophen-2-yl)-2,5-dihydrop yrrolo[3,4-c]pyrrole-1,4-dione) (coded as H1), which used diketopyrrolopyrrole as terminal functionalities, was designed, synthesized and characterized. H1 displayed a very high optical absorption coefficient, good solubility and thermal stability, promising optoelectronic properties, and high electron mobility, and afforded an encouraging efficiency of 5.42% when paired with the archetypal electron donor poly(3-hexylthiophene).
In recent years, there has been a dramatic surge in the development of non-fullerene acceptors and research has indicated that thoughtfully designed target chromophores may rival the development of donor functionalities. Recent reports, for instance D. Meng et al.,6 Y. Lin et al.,7 Hwang et al.,8 Zhong et al.9 and A. Rananaware et al.,10 have not only demonstrated encouraging efficiencies but have shown unique structural formats to be used as non-fullerene acceptors. Although recent advances in the design and development of non-fullerene acceptors have been impressive,11 there still remains the need to develop materials which not only will have better properties in terms of solubility, stability, and strong accepting strength but have energy levels matching those of the conventional and conjugated polymeric and small molecular donor functionalities. Furthermore, in order to make these acceptors viable for practical applications, they must be easily synthesizable and be electronically and physically compatible with the commercially available donors, such as poly(3-hexylthiophene) (P3HT).
The design of most efficient and promising small molecular non-fullerene acceptors indicates that a target chromophore should be a conjugated structure, either through a combination of various building blocks (primarily donors and acceptors) or through the possession of a rigid, extended fused-ring backbone.7,8,10 With such criteria in mind and learning from the work reported by us and others, we also thought to evaluate unique structural formats. We observed that functionalities such as diketopyrrolopyrrole (DPP) and naphthalene diimide (NDI) are strong accepting units that can be integrated with other conjugated blocks, either donors or acceptors, and can generate targets that can fulfil most of the demanding requirements of efficient non-fullerene acceptors. The use of DPP, in particular, appealed to us as the chromophores bearing terminal DPP units (1) can achieve higher Voc, (2) are soluble in most of the common processing solvents, (3) exert good thermal and chemical stability, and (4) can be generated with simple, facile and easily scalable synthetic strategies. Such advantages are likely to be responsible for prompting interest in the design of chromophores based on terminal DPP units and the overall development of novel non-fullerene acceptors based on DPP functionality.
Fig. 1 reveals the molecular structure of the novel, H-shaped, small molecular non-fullerene electron acceptor, 6,6′,6′′,6′′′-([9,9′-bifluorenylidene]-2,2′,7,7′-tetrayltetrakis(thiophene-5,2-diyl))tetrakis(2,5-bis(2-ethylhexyl)-3-(thiophen-2-yl)-2,5-dihydropyrrolo[3,4-c]pyrrole-1,4-dione) (coded as H1), which was designed based on the central bifluorenylidene and terminal diketopyrrolopyrrole functionalities. The molecule H1 is a highly conjugated chromophore, which was designed by taking into account most of the structural requirements of an efficient non-fullerene acceptor. It is important to point out that the central 9,9′-bifluorenylidene (BF) functionality was reported by F. G. Brunetti et al. as a new generation of acceptor compounds for organic electronic applications.12 More recently, K. Rakstys et al. have reported the use of the BF functionality for a different type of photochemical cell, known as a perovskite cell.13 The proposed design of H1, which includes a combination of potential BF and DPP functionalities, provided solution-processable BHJ devices based on the blend of P3HT:H1 (1:1 w/w), which affords a promising efficiency of 5.42% with a high Voc of 1.17 V. These efficiency and Voc values are among the highest numerals for a single-junction BHJ device incorporating a non-fullerene acceptor and the common donor polymer P3HT. This current work is a continuation of our efforts made in the design and development of small molecular chromophores for organic photovoltaic applications.14
Fig. 1 Molecular structure of the newly designed and synthesized non-fullerene electron acceptor H1. |
Fig. 2 shows the normalized spectra of optical absorption of H1 in chloroform solution, and in as-cast thin and blend films. In solution, H1 displayed a very high optical absorption coefficient (∼91000 L mol−1 cm−1 at 5.17 μM). A pristine film of H1 revealed significant absorption throughout the visible region (350–800 nm) with two peaks at 408 and 599 nm, and the longest wavelength absorption maximum (λmax) was red shifted by 10 nm compared to its solution λmax. The blend film using a combination of P3HT/H1 (1:1) demonstrated strong light-harvesting ability over the entire visible zone, thus suggesting that there is an efficient charge transfer transition between the donor and acceptor domains. Furthermore, the photoluminescence studies were carried out on both the pristine and blend films of H1. The photoluminescence quenching measurement can provide valuable insight into the ability of the donor–acceptor interface to dissociate excitons. The presence of P3HT in the as-cast, blend films of P3HT:H1 (1:1 w/w) quenched the photoluminescence (Fig. S1 in ESI†), thus indicating that an efficient photo-induced charge transfer occurs between H1 and P3HT in the blend film. This is further indicative of a more intimately mixed blend morphology.
Density functional theory (DFT) calculations using the Gaussian 09 suite of programs15 and the B3LYP/6-311+G(d,p)//B3LYP/6-31G(d) level of theory indicated that the highest occupied molecular orbital (HOMO) and the lowest unoccupied molecular orbital (LUMO) densities are well segregated, a finding that assures an efficient charge transfer transition (Fig. 3). DFT calculations further revealed that the torsional angles between the internal thiophene ring planes (of DPP) and phenyl ring planes (of BF) were ∼20° and 50°, thus pointing out that H1 is a highly non-planar structure overall (Fig. S2, ESI†).
The central double bond joining the two fluorene components is twisted and is under strain. Calculations show it to be longer than a normal double bond (1.382 Å vs. standard 1.340 Å), indicating that it is under strain and primed for reduction. Given the precedence of research by Brunetti and Wudl12, which describes highly twisted double bonds between various aromatic structures and their ability to accept electrons, we would expect H1 to be similarly activated toward accepting an electron to relieve strain and increase aromaticity in the fluorene systems (angle twist in H1 = 40°). Once an electron is accepted, the radical anion formed will be stabilized, with the radical delocalized in one-half of the molecule and the anion delocalized in the other. In addition, non-planar molecular formats can be desirable for designing a potential non-fullerene acceptor, mainly due to the fact that such arrangements can prevent strong intermolecular aggregation whilst sustaining broadened conjugation in each direction for photon harvesting. We and others have recently demonstrated this principle while designing efficient non-fullerene electron acceptors.10,11a The experimental estimation of the HOMO energy level was carried out using photoelectron spectroscopy in air (PESA), and the LUMO level was calculated by adding the optical band gap (film spectrum) to the HOMO value. The HOMO and LUMO values were found to be −5.51 eV and −3.84 eV, respectively, thus suggesting that H1 is a low band gap material. Appropriately positioned energy levels of H1 suggested that it can certainly achieve a high Voc when fabricated using the conventional donor polymer P3HT. Theoretical calculations also revealed that H1 exerts a low band gap and a high HOMO level of 1.82 eV and −5.18 eV, respectively, a result that provides strong support to our experimental findings (Fig. S3, ESI,† for the PESA curve and Fig. 4 for the energy level diagram). The theoretical optical absorption transitions of H1 were also calculated and corroborated our experimental findings (Fig. S4, ESI†). We further realised that not only should organic semiconductors be highly soluble and chemically stable, they should also be thermally stable for allowing device processing, such as annealing, if required. Keeping this criterion in mind, we conducted thermogravimetric analysis (TGA). TGA demonstrated that the thermal stability of H1 is excellent (for TGA curve see Fig. S5, ESI†).
Fig. 4 Energy level diagram showing alignments of different components of the BHJ device architecture. |
Once it had been established that H1 displayed appropriate optoelectronic properties, we evaluated its performance as a non-fullerene electron acceptor along with the classic electron donor P3HT in solution-processable BHJ devices under simulated sunlight and monochromatic light illumination. Solar cells using a conventional configuration of indium tin oxide (ITO)/poly(3,4-ethylenedioxythiophene):poly(styrene-sulfonate) (PEDOT:PSS, 38 nm)/active layer (∼68 nm)/Ca (20 nm)/Al (100 nm) were fabricated, where the active layer was a 1:1 blend of P3HT:H1, spin-cast from o-dichlorobenzene on top of the PEDOT:PSS-coated substrate. Control devices based on P3HT:PC61BM were also fabricated. We chose a simple device architecture to start with, and observed the initial performance, stability, fabricating conditions and reproducibility of the BHJ devices. With regard to the fabrication of fullerene-free organic solar cells, it is becoming evident that the use of a high boiling point solvent, for instance dichlorobenzene, may affect device performance. The recent literature reported by us and others demonstrates such considerations.16 Based on such principles and our own understanding of the BHJ device architecture, the active films were spin-coated from o-dichlorobenzene solutions (1:1 donor:acceptor w/w).
The current density–voltage (J–V) curves of the devices (with a D/A weight ratio of 1:1) under different conditions measured under 100 mW cm−2 simulated sunlight illumination are shown in Fig. 5. The best as-cast device (device area = 0.1 cm2; a total of six devices were made) showed an impressive PCE of 5.42%, with a Voc of 1.17 V, a short-circuit current density (Jsc) of 7.74 mA cm−2 and a fill factor (FF) of 0.60. However, thermal annealing, for instance 100 °C for 10 minutes, of the active surface exerted an adverse effect on the device performance and the PCE dropped by approximately 50%. We noticed that this inferior photovoltaic performance was primarily due to the low film quality, where we physically observed roughness and minor cracks on the active surface after thermal annealing. Similar poor performance was observed for other D:A combination, for example 1:1.5, indicating that the 1:1 combination in the current study is the best possible combination in order to achieve high device outcome. Our physical observation of the 1:1 combination (pre- and post-annealing film) was supported by an atomic force microscopy (AFM) analysis, which was conducted in tapping mode, where the surface roughness was more than doubled when compared to the unannealed surface, thereby indicating an irregular mixing of donor and acceptor domains (Fig. 6). The annealed device exhibited a PCE of 2.32%. In contrast, the maximum PCE reached 3.01% for a controlled device based on P3HT:PC61BM.
The devices with H1 as an acceptor exhibited much higher Voc than the devices with PC61BM as an n-type semiconducting component (1.17 V vs. 0.56 V). The higher Voc in the case of H1 is consistent with the measured optical band gap between the LUMO of H1 and the HOMO of P3HT. Not only is H1 the first reported example in the literature where the amalgamated use of BF and DPP functionalities has been carried out to generate an efficient, H-shaped non-fullerene electron acceptor, but the PCE value reported here is among the highest values reported for P3HT and small molecular non-fullerene electron acceptor solar cells fabricated using a simple device architecture. The results achieved in the current work validate the use of an H-shaped or non-planar molecular format as a favourable structural concept for the design and development of highly efficient, small molecular non-fullerene acceptors for BHJ devices (see Table S1, ESI,† for detailed device parameters).
The incident photon-to-current conversion efficiency (IPCE) measurement of the blended film with a D/A weight ratio of 1:1 is shown in Fig. 7. The blended film of the best photovoltaic device showed a broad IPCE spectrum ranging from 350 to 800 nm, typically over the entire visible region, with an IPCE maximum of approx. 42% at 596 nm. Apparently, the broadness of this IPCE spectrum suggests that H1 is a type of electron acceptor that can be blended with a variety of electron donors, for example conjugated polymers and small molecular donors, in order to achieve charge generation over a broad range of wavelengths. Photocurrents obtained from the IPCE data are in close agreement with those of current–voltage measurements.
Fig. 7 The IPCE curve of the best performing device described in Fig. 5 (H1 = IPCE spectrum of P3HT:H1 blend and H1 B Abs corresponds to P3HT:H1 blend absorption). |
The study of the actual surface morphology of the blend films of P3HT:H1 (1:1 w/w) is shown in Fig. 6. As mentioned above, the unannealed blend showed a smooth surface morphology with a root-mean-square (RMS) roughness of 3.6 nm, while the P3HT:H1 annealed blend displayed an RMS roughness of 8.6 nm. Although the blend surfaces indicated a strong domination of P3HT controlling the surface morphology, the unannealed blend appeared to be well interlaced, which is advantageous for exciton dissociation and can result in an enhanced efficiency of photovoltaic devices. Such a well-plaited surface was further confirmed by transmission electron microscopy (TEM) analysis, where we were able to observe a finer texture. This usually results in relatively higher values of Jsc and FF (Fig. 8). To gain insight into the effective charge carrier mobilities, the space charge limited current (SCLC) method was applied to get information about the charge transportation in the devices. The electron-only devices, consisting of an active layer sandwiched between a ZnO coated ITO electrode and LiF/Al counter-electrode as the hole-blocking contact, were fabricated as per the sketch depicted in Fig. S6, ESI.† From the current density as a function of the voltage data (Fig. S7, ESI†), the electron mobility in the trap-free SCLC region can be estimated using the Mott–Gurney equation [(J = 9(εμ)/8 × (V2/d3)), where ε is the dielectric constant, μ is the charge-carrier mobility, d is the sample thickness, and V is the applied voltage]. Using this expression, an excellent electron mobility of the order of 10−3 (2.40 × 10−3 cm2 V−1 s−1) was observed, which is beneficial for achieving higher Jsc and FF values with the resulting OPV devices.
Details of spectroscopic measurements, as well as device fabrication and characterization of photovoltaic devices, have been reported previously.14a,b,e,f AFM topographic maps were performed directly on the active layer of the P3HT:H1 blends using an Asylum Research MFP-3D-SA instrument. The AFM was run in intermittent contact mode (tapping mode) using MikroMasch NSC18 tips with a typical resonant frequency of ∼100 kHz, a typical probe radius of ∼10 nm, and a typical aspect ratio of 3:1. TEM samples were prepared by solvent evaporation on a holey carbon grid and micrographs were produced using a JOEL 1010 100 kV TEM.
The synthesis of 6,6′,6′′,6′′′-([9,9′-bifluorenylidene]-2,2′,7,7′-tetrayltetrakis(thiophene-5,2-diyl))tetrakis(2,5-bis(2-ethylhexyl)-3-(thiophen-2-yl)-2,5-dihydropyrrolo[3,4-c]pyrrole-1,4-dione) (H1) was performed as follows. To a stirred solution of 2 (488 mg, 0.75 mmol) in a solvent mixture of toluene:t-butanol:tetrahydrofuran (1:1:1) (30.0 mL) was added K2CO3 (103 mg, 0.75 mmol) and the resultant reaction mixture was degassed for 15 min followed by the addition of tetrakis(triphenylphosphine)palladium (0) (43 mg, 30 mol%). The resulting suspension was stirred for 30 min under a nitrogen atmosphere followed by the addition of compound 1 (80 mg, 0.124 mmol), and the cherry-coloured reaction mixture was stirred at 100 °C for 48 h. The reaction mixture was quenched with water and extracted with chloroform (3 × 30 mL). The combined organic layers were washed with water followed by brine, dried over anhydrous MgSO4 and concentrated under vacuum to produce a crude residue, which was purified by traditional column chromatography (hexane:diethyl ether 9:1) to afford H1 as a light bluish solid with a metallic lustre (120 mg, 41%); 1H NMR (400 MHz, CDCl3) δ 8.92 (dd, J = 3.9, 1.1 Hz, 1H), 8.88 (d, J = 3.8 Hz, 1H), 8.41 (d, J = 1.6 Hz, 1H), 7.71 (d, J = 3.9 Hz, 1H), 7.63 (dd, J = 5.0 Hz, 1.2 Hz, 1H), 7.56–7.50 (m, 2H), 7.29–7.27 (m, 1H), 4.08–4.00 (m, 4H), 1.87–1.83 (m, 2H), 1.34–1.22 (m, 16H), 0.89–0.83 (m, 12H); 13C NMR (100 MHz, CDCl3) δ 162.67, 142.32, 142.08, 141.17, 141.01, 140.13, 139.89, 139.38, 139.30, 138.93, 138.40, 137.56, 137.34, 132.28, 130.62, 130.37, 130.06, 128.95, 128.83, 128.51, 124.17, 108.26, 45.94, 39.25, 36.62, 31.58, 30.31, 23.22, 14.18, 10.59; MALDI-TOF (m/z) [M]+ 2417.1; found for C146H168N8O8S8. Elemental analysis calculated for C146H168N8O8S8 (%): C 72.48, H 7.00, N 4.63; found C 72.45, H 6.96, N 4.61.
Footnote |
† Electronic supplementary information (ESI) available: PL, theoretical optical absorption, PESA, TGA and SCLC curves, and experimental spectra. See DOI: 10.1039/c7qm00084g |