Maoquan Xue*a,
Zhiping Wanga,
Feng Yuana,
Xianghua Zhangb,
Wei Wei*c,
Hua Tangd and
Changsheng Lid
aChangzhou Vocational Institute of Light Industry, Changzhou, Jiangsu Province 213164, P. R. China. E-mail: xuemaoq@163.com
bSchool of Mechanical Engineering, Jiangsu University of Technology, Changzhou, Jiangsu Province 213001, P. R. China
cSchool of Materials Science and Engineering, Changzhou University, Changzhou, Jiangsu Province 213164, P. R. China. E-mail: benjamin.wwei@163.com
dSchool of Materials Science and Engineering, Jiangsu University, Zhenjiang, JiangsuProvince 212013, P. R. China
First published on 17th January 2017
TiO2/Ti3C2Tx hybrid nanocomposites were successfully prepared by a facile liquid phase synthesis technology. The phase structure and morphology of as prepared samples were analyzed by means of X-ray diffraction and scanning electron microscopy. The results revealed that uniform TiO2 particles were distributed within the surface and edge of Ti3C2Tx nanosheets. Subsequently, the tribological properties of the TiO2/Ti3C2Tx hybrid nanocomposite as lubricant additive in base oil were evaluated with a UMT-2 ball-on-disc tribotester, and the morphologies of worn steel surfaces were investigated using a scanning electron microscope and non-contact optical profile testing instrument. The results of the friction tests showed that base oil with 1 wt% TiO2/Ti3C2Tx hybrid nanocomposite under optimal load had excellent friction reduction. The morphology of the worn surface analyzed by SEM and non-contact optical profile testing confirmed that the hybrid nanocomposites mended the scratched surface and formed a uniform tribofilm, thereby helping to improve the tribological properties of the base oil. Furthermore, this work shows the promising applications of TiO2/Ti3C2Tx hybrid nanocomposites in the field of tribology.
The laminated structure of Ti3AlC2 is comprised by alternative stacking of hexagonal TiC layers and congested edge-sharing bidimensional Al atomic layers along the c-axis, in which the bonding between Ti and C is firmly covalent, but the metallic bonding between Ti and Al is comparatively weak and therefore more susceptible to chemical reaction.14–16
Lately, Naguib et al.17,18 reported to fabricate two-dimensional Ti3C2(OH)2 nanosheets by selectively etching the Al layers with hydrofluoric acid (HF), following a similar process, other MAX phases have also been successfully exfoliated into the two-dimensional transition metal nanocarbides and nanonitrides named Mxenes,19–21 theoretical and experimental investigation revealed that their properties distinct from those of their 3D MAX counterparts.22–29
Over the past decades, TiO2, as a typical member of inorganic transition metal dioxides, has aroused numerous studies due to its attractive functional properties and promising applications. Furthermore, various hybrid modifications including surface modification, coupling with porous materials, and carbon coating have been executed to TiO2 nanostructures in order to improve the properties. At present, several attempts have been made in the syntheses and properties of TiO2 hybrid nanostructures. Soraya Hosseini et al.30 studied the mesoporous carbon and TiO2 photoanodes synthesized by sol–gel spin coating onto a glassy substrate, and found that the enhanced humic acid removal of TiO2/C/C/TiO2 photoanodes was due to the highest photocurrent density generated. Hong Z et al.31 fabricated the TiO2@C–rGO hybrid nanostructures through in situ growth of oriented self-assembly of TiO2 mesocrystals on GO route, the hybrid nanostructures display a high reversible capacity, superior rate capability, and long term cycling stability, which is largely attributed to the strong architecture of well-dispersed carbon-coated mesoporous TiO2 mesocrystals anchored on conductive graphene network. Wongaree M et al.32 prepared CNT/TiO2 nanofibers by spinning CNT/poly(vinyl pyrrolidone) (PVP) solution followed by the removal of PVP, the synergistic effects of the larger surface area and lower band gap energy of CNT/TiO2 nanofibers were presented as robust adsorption ability and greater visible light adsorption. Qian L et al.33 produced biomorphic charcoal/TiO2 composites from moso bamboo templates, the C/TiO2 composites were exhibited lower geometrical density, better thermostability, and favorable microwave absorptive properties. Naguib M34 and Gao35 et al. fabricated TiO2/C nanohybrids by mild oxidation of Ti3C2, the obtained samples were exhibited extremely high cycling rates when tested as anodes and good photocatalytic activity. However, TiO2/Ti3C2Tx hybrid nanostructures and their application in the tribiological field have rarely been reported.
In this work we report a simple method to prepare TiO2/Ti3C2Tx via immersing Ti3C2Tx powders in distilled water assisted hydrothermal reaction. Moreover, the tribological properties of TiO2/Ti3C2Tx composites as additives in the base oil were also investigated. This study will be useful for Mxene practical application in the future.
To exfoliate the Ti3AlC2 to Ti3C2Tx (Mxenes), 5 g Ti3AlC2 powders was immersed in a 40 wt% aqueous hydrofluoric acid solution, and magnetically stirring for 100 h at room temperature. Afterwards the etched powder mixtures were filtered and washed with ethanol and distilled water several times, and dried to obtain Ti3C2Tx powders.
TiO2/Ti3C2Tx hybrid nanostructures were synthesized using a hydrothermal process. The prepared Ti3C2Tx was added to distilled water and stirring evenly, then the solution was transferred to a Teflon-lined autoclave and placed in an electric oven heated at 200 °C for different time. After the hydrothermal process, the as-prepared product was washed with distilled water and ethanol for several times and then dried at 60 °C for 12 h. Finally, black powders were obtained.
The size and morphology of Ti3AlC2 sample were identified by SEM. Fig. 1b shows the SEM images of the as-prepared Ti3AlC2 sample. Fig. 1b reveals that the sample consists of a lot of densely aligned laminated-like structure and smooth surface. Further observation shows that the particles have melting imprint, indicating the formation of liquid phase at high temperature,3 the result indicating that high-yield and good morphology of Ti3AlC2 could be readily achieved through this approach.
Fig. 3I gives the XRD patterns of the exfoliated Ti3C2Tx powders obtained by 40% HF treatment. After HF treatment, the labelled diffraction peaks in Fig. 3I can be indexed to those of the phase of Ti3C2Tx and TiC,17 the peaks indexed to Ti3AlC2 have clearly vanished. The XRD patterns of product verify the formation of Ti3C2Tx phase.28,36,37 The strong peaks were found around 9.0° and 18.2° corresponding to (002) and (004) of Ti3C2Tx, which shift to lower 2θ angles contrasting to the diffraction of Ti3AlC2, manifesting the expansion along c-axis. Owing to the weak metallic bonding between Ti and Al, the Al layer is exfoliated by selective etching off Ti3AlC2.28 SEM images (Fig. 2) show that the obtained samples are uniform separated layers with an average thickness of about 10 nm.
Fig. 3 gives the X-ray diffractograms of Ti3C2Tx before and after hydrothermal treatment in distilled water at 200 °C. The XRD patterns of the products of Ti3C2Tx after treatment at 200 °C for 12 h can be indexed for both TiO2 and Ti3C2Tx, in addition, it also can be clearly seen that the intensity of TiO2 peaks increased as the reaction time increasing, while the fraction of not oxidized Ti3C2Tx was greatly reduced. This reveals the kinetics of the oxidation process as a carbide consuming mechanism.34
Fig. 4 exhibits a typical SEM images for Ti3C2Tx sample treated at 200 °C for 24 h. It can be seen from Fig. 4a that there are many uniform oxide particles distributing within the surface and edge of the thinner layers, while the original microstructure of Ti3C2Tx is separately layered structure (Fig. 2). The magnified SEM image (Fig. 4b) further gives the details of hybrid nanocomposite. There are significant amounts of TiO2 co-exist with Ti3C2Tx, the size of TiO2 particles is about 100 nm.
Fig. 4 SEM images of Ti3C2Tx after hydrothermal treatment in water at: (a) 200 °C for 24 h, and (b) zoom in on the region framed in (a). |
In order to discuss the evolutions of the friction coefficients of TiO2/Ti3C2Tx hybrid nanocomposites, the concentration of the nanocomposites in the lubricant was studied. Several concentrations in the range from 0.6 wt% to 5 wt% were chosen. And the tests were carried out with 20 N, 150 rpm, 600 s and the room temperature, respectively. The friction coefficients of the tests are offered in Fig. 5a. It can be seen that under base oil lubrication, the friction coefficient has a decreasing trend over 300 s, and then stabled with an average value of 0.103. The base oil with 0.6 wt% TiO2/Ti3C2Tx hybrid nanocomposites lubrication has the same trend with the base oil lubrication, maintained a friction coefficient of approximately 0.075 after 300 s sliding. The base oil with 1 wt% TiO2/Ti3C2Tx lubrication showed the lowest friction coefficient of 0.073 with a slight decreasing trend. This may be because, with the continuous sliding, more and more TiO2/Ti3C2Tx were adhered to the friction surfaces creating a tight layer between the two contact surfaces, leading to a reducing friction coefficient. However the friction coefficient of base oil with 3 wt% concentration became erratic and lifted along sliding time after 150 s sliding. When the base oil formulated with 5 wt% TiO2/Ti3C2Tx, the friction coefficient rose observably over 0.16 and an increasing trend with sliding time.
When the concentration of TiO2/Ti3C2Tx hybrid nanocomposites is 1 wt%, the best antifriction performance is achieved. The remarkable tribological property may due to their TiO2 nanoparticles and thin laminated structure. Furthermore, the nanoparticles can readily enter into the boundary with base oil and form a uniform shielded film, so the behavior of friction coefficient is more steady than others, but too much higher concentration of the nanoparticles revealed vast agglomeration, could not enter the contact area easily,38,39 also could damage the consistency of the gluey system of the base oil.40 So, the optimum concentration of the TiO2/Ti3C2Tx hybrid nanocomposites as an additive in base oil is proposed to be 1 wt%.
Fig. 5b reveals the change of friction coefficient of 1 wt% TiO2/Ti3C2Tx hybrid nanocomposites as an additive of lubricant under different loads, respectively. It can be observed that there is a trend that the friction coefficient of nanocomposites decreases firstly and then increases as the load increases, also, the curves of 30 N and 50 N have higher undulation than the curves of 5 N and 20 N. We can get the ideal load for friction display at 20 N. Within the scope of certain pressure, TiO2/Ti3C2Tx hybrid nanocomposites is delaminated readily at the contact region and precipitate a tribofilm, which can reduce shearing stress and generate a low friction coefficient. When the applied load is 5 N, TiO2/Ti3C2Tx cannot be compacted on the friction surface to repair grinding crack, so the protective film was not shaped. Otherwise, if the applied load is too high, the protective film at the region will be damaged, finally inducing high undulation and friction coefficient.
With the aim of study the wear resistance performance of TiO2/Ti3C2Tx hybrid nanocomposites as lubricant oil additives, the grinding cracks of plate after friction were examined by SEM and BRUKER ContourGT non-contact 3D optical profile testing apparatus.
SEM photographs of the worn scar lubricated by base oil with different concentrations of TiO2/Ti3C2Tx hybrid nanocomposites under 20 N are given in Fig. 6 and 7a. Fig. 6a presents that the rubbed surface lubricated by the pure base oil is quite rough with lots of wide and deep furrows along the sliding direction because of contact fatigue. In Fig. 6b and 7a, the worn surface lubricated with base oil added 0.6 and 1.0 wt% TiO2/Ti3C2Tx hybrid nanocomposites is smoother than that lubricated with pure base oil. The furrows are shallower and subtler on the worn surface of steel disc under the lubrication of base oil with 0.6 and 1.0 wt% TiO2/Ti3C2Tx, meanwhile, a thin tribofilm is formed on the substrate. However, the wear scar becomes obviously rough and the plastic deformation is severe when 3.0 wt% and 5.0 wt% TiO2/Ti3C2Tx were added into the base oil, which is well corresponded to the unstable and higher friction coefficient, as shown in Fig. 5a. It can be inferred that the tribological properties of the base oil could be significantly improved by adding the TiO2/Ti3C2Tx hybrid nanocomposites as additives, though the content of TiO2/Ti3C2Tx must be controlled at a reasonable level. Too much TiO2/Ti3C2Tx may act as superfluous abrasive particles and result in the deterioration of the friction conditions.
Fig. 6 SEM images of the grinding cracks lubricated by base oil with different concentrations 0 wt% (a), 0.6 wt% (b), 3.0 wt% (c), and 5.0 wt% (d) hybrid nanocomposites. |
Fig. 7 SEM images of the grinding crack lubricated by base oil with 1.0 wt% TiO2/Ti3C2Tx hybrid nanocomposites under (a) 20 N and (b) 50 N. |
The morphology of the grinding crack lubricated by base oil with 1 wt% TiO2/Ti3C2Tx hybrid nanocomposites under 20 N and 50 N was observed using SEM, as revealed in Fig. 7. This SEM image in Fig. 7a shows that the friction surface lubricated by the base oil with 1 wt% TiO2/Ti3C2Tx hybrid nanocomposites under 20 N is glossy. The furrows are shallow and no distinct mechanical damage on the worn surface of steel disc, meanwhile, a light tribofilm is shaped on the substrate. However, under the load 50 N, as shown in Fig. 7b, the worn surface proves clearly coarse and the plastic deformation is rigorous, which is consistent with the higher and labile friction coefficient, as shown in Fig. 5b.
Fig. 8 illustrates grinding crack of the base oil with 1 wt% TiO2/Ti3C2Tx hybrid nanocomposites at 150 rpm for 600 s under the load of 20 N and 50 N. It can be distinct observed that the grinding crack under 20 N is composed of glossy and shallow furrows along the sliding direction (Fig. 8a), and the grinding crack caused by under 50 N (Fig. 8b) is wider and distributed irregular pits. From the images we can see that the depth and width of the wear scar for 20 N are about 30 μm and 280 μm respectively, while those for 50 N are about 35 μm and 400 μm. This manifests that the base oil with TiO2/Ti3C2Tx hybrid nanocomposites under 20 N shown better anti-wear ability than 50 N.
Fig. 8 Non-contact 3D optical profile testing instrument images of the grinding crack of the base oil with 1 wt% TiO2/Ti3C2Tx hybrid nanocomposites under (a) 20 N and (b) 50 N. |
The tribological tests and morphology of the grinding crack results suggest that the 1 wt% TiO2/Ti3C2Tx nanocomposites with the optimal load (e.g., 20 N) aids to form continuous and uniform tribofilm on the rubbing surface leading to friction reduction.
The tribological mechanism between the rubbing surfaces in base oil with TiO2/Ti3C2Tx hybrid nanocomposites is iconically presented in Fig. 9. It is believed that the suitable content of TiO2/Ti3C2Tx hybrid nanocomposites under appropriate load could enter in the gap between the friction surfaces easily. During sliding, the desquamated TiO2 particles can mending the scratched surface to decrease the contact of rough between the friction surfaces, meanwhile the exfoliated Ti3C2Tx sheets adsorb onto the rubbing surface and form a tribofilm, which can decrease shearing stress and the direct contact of tribopair, this is the main mechanism for improving the tribological behavior of TiO2/Ti3C2Tx hybrid nanocomposites.
This journal is © The Royal Society of Chemistry 2017 |