Open Access Article
This Open Access Article is licensed under a
Creative Commons Attribution 3.0 Unported Licence

Leaching of fluorine and rare earths from bastnaesite calcined with aluminum hydroxide and the recovery of fluorine as cryolite

Jingui Heab, Yong Lia, Xiangxin Xue*a, Hongqiang Rub, Xiaowei Huangc and He Yanga
aSchool of Metallurgy, Northeastern University, Shenyang, Liaoning 110819, China. E-mail: xuexx@mail.neu.edu.cn; Xue_Xiangxin@126.com
bSchool of Material Science and Engineering, Northeastern University, Shenyang, Liaoning 110819, China
cNational Engineering Research Center for Rare Earth Materials, General Research Institute for Nonferrous Metals and Grirem Advanced Materials Co., Ltd., Beijing 100088, China

Received 12th December 2016 , Accepted 22nd February 2017

First published on 2nd March 2017


Abstract

In order to avoid fluorine loss and contamination, and recover the fluorine resource in bastnaesite, a new process of decomposing bastnaesite with aluminum hydroxide followed by sulfuric acid leaching was proposed. The calcination mechanism was discussed by TG-DSC and XRD analyses. Fluorine could be taken up by Al2O3, and the discharge of fluorine was prevented. Leaching from calcined ore was achieved with dilute sulfuric acid, and the parameters affecting the leaching rates of fluorine and rare earths (REs) were investigated. It shows that the leaching rates of F, Ce and total RE of 92.71%, 98.92% and 98.61% could be obtained under the conditions of n(Al)/n(F) 1/2, calcination temperature 500 °C, calcination time 1 h, sulfuric acid concentration 3 mol L−1, leaching temperature 90 °C and leaching time 1 h. Fluorine could be separated from REs after extraction, and was recovered as Na3AlF6 with the recovery rates of fluoride and aluminum greater than 96%. XRD and SEM analyses indicated that the monoclinic phase cryolite was obtained.


1 Introduction

Bastnaesite constitutes one of the principal rare earth minerals of light rare earths in China with the chemical formula RECO3F or RE2(CO3)3·REF3 (RE = rare earth), which theoretically contains 50% cerium, 0.2–0.3% thorium and 8–10% fluorine, etc.1–3 It is mainly distributed in Baiyunebo of Inner Mongolia, Mianning of Sichuan Province and Weishan of Shandong Province.4 A series of efficient hydrometallurgical technologies have been developed to process bastnaesite. At present, the main methods for processing bastnaesite in industry include a concentrated hydrochloric acid leaching–alkali conversion method, oxidation calcination–acid leaching method, etc. The concentrated hydrochloric acid leaching–alkali conversion method is used to produce CeO2 and less-Ce mixed RE chloride. This method is unfriendly to the environment due to the volatilization of concentrated hydrochloric acid solution and the discharge of fluorine and the radioactive element thorium. The oxidation calcination–hydrochloric acid leaching method is commonly used for the smelting of bastnaesite by rare earth enterprises.5 During the calcination process, bastnaesite can be broken down into rare earth oxides and rare earth oxyfluorides, and the Ce3+ is mostly oxidized to Ce4+. The Ce4+ can be separated from the other RE3+ when hydrochloric acid is used to leach calcined ore. The leaching residue rich in Ce4+ can be collected and used to produce high-purity cerium products. However, this method has many shortcomings such as discharge of fluorine-containing wastewater, low rare earth recovery, serious environmental pollution and long process flow.6 The oxidation calcination–sulfuric acid leaching–solvent extraction process can recover most of the rare earths and bearing valuable elements, and has rapid dissolution speed and high leaching rate, making it a more advanced technology for smelting of bastnaesite.7–9 However, some issues still remain resulting from the existence of 8–10% fluorine. Some of fluorine escapes as hydrogen fluoride gas from the decomposition of bastnaesite in the oxidation calcination process as well as in the leaching process, and also part of fluorine is left in the residue as insoluble fluorides in the sulfuric acid leaching process.4,10 In recent years, annual treated quantity of bastnaesite was about 22[thin space (1/6-em)]500 tons, thus, a great quantity of fluorine was produced and discharged into the environment, which will lead to serious pollution of surface and ground water.11 Fluoride has been listed as one of the contaminants in water by the World Health Organization (WHO), which will cause many problems in human health. Therefore, fluorine contamination is considered as a serious pollution worldwide.12 Fluorine is also an important strategic resource, thus, the discharge of such waste is a waste of fluorine resource. After leached by sulfuric acid, fluoride mainly exists as [CeF2]2+ in leaching solution, which makes it difficult to separate F and Ce4+, leading to the formation of the third phase in the extraction of rare earths.13–15 Considering the problems caused by fluorine, some new defluorination smelting technologies of bastnaesite have been explored, such as NH4Cl roasting method,16 Na2CO3 roasting method17 and CaO roasting method.4 However, these methods have their own shortcomings, such as multiple washing and solid–liquid separation steps, production of large amount of fluoride-containing wastewater and residue which are difficult to treatment, large energy consuming and high investment; therefore, they are rarely applied in industrial production. Wang et al.18 invented a new method to recover fluorine. Firstly fluoride was extracted into the organic phase as [CeF2]2+, then the strip liquor containing aluminum salt was utilized to scrub fluoride from the F and Ce4+ loaded organic phase. This technology does not involve the elimination and recycling of discharged hydrogen fluoride waste gas in the oxidation calcination and leaching processes as well as the recovery of insoluble fluorides in bastnaesite. In addition, some Al3+ will enter into the organic phase, resulting in a substantial organic consumption.

Fluoride is considered as a hard base because of the small ionic size and high electronegativity, which possesses a strong affinity for metal ions such as Al3+, B3+ and Fe3+. Our lab has conducted the exploration of using boron salts and aluminum salts as defluoridation reagent in fluoride-bearing rare earths sulfate solution.19 To solve the problems of fluorine loss and contamination, and recover the fluorine resource in bastnaesite, a new process of decomposing bastnaesite with aluminum hydroxide was proposed in this study. The discharge of fluorine can be prevented by converting the fluorine into aluminum fluoride. Leaching for calcined ore was performed with dilute sulfuric acid. Then, the rare earths in the leaching solution were extracted by di-(2-ethylhexyl) phosphoric acid (HDEHP), and the raffinate containing aluminum fluoride was used to recover fluorine as cryolite (Na3AlF6). The cryolite is an essential chemical material and is widely used in industry, particularly in the Hall–Héroult process (a process for aluminum production).20 This paper aims to avoid the fluorine pollution through reducing the discharge of waste containing fluorine, recover the fluorine resource in bastnaesite and eliminate the negative influence of fluorine on the extraction of rare earths.

2 Experimental

2.1 Materials and apparatus

All reagents and organic solvents used were of analytical grade. Aluminum hydroxide, sodium fluoride, sodium hydroxide etc. were supplied by Guoyao Group Chemical Reagent Shenyang Co., Ltd. The sulfuric acid (98%) was supplied by Shenyang Laibo Kemao Co., Ltd. HDEHP and kerosene were supplied by Shanghai Rare-earth Chemical Co., Ltd. and used without further purification. The bastnaesite samples used were obtained from Mianning mine of Sichuan Province in China. The chemical compositions are given in Tables 1 and 2.
Table 1 The main chemical composition of bastnaesite (wt%)
Component RExOy F CaO SrO Fe2O3 BaO SiO2
Content/% 62.22 8.92 7.29 6.43 5.42 3.75 1.79


Table 2 The main RE distribution of bastnaesite (wt%)
Component CeO2 La2O3 Nd2O3 Pr6O11 Sm2O3
Content/% 31.51 23.33 5.26 1.92 0.23


WLS-5 rapid intelligent muffle furnace (Hebi Tianhong Instrument Co., Ltd.) was utilized to conduct calcination experiments. ZXS100e X-ray fluorescence spectrometer (XRF) (Rigaku) was utilized to detect the compositions of samples. PW3040/60 X-ray diffraction (XRD) instrument (Panalytical) was utilized to determine the phase composition of samples in the 2θ of 10–80° with Cu Kα radiation, at a scan speed of 4° min−1 and a step size of 0.02°. SDT 2960 thermal analyzer (TA instruments) was utilized to measure the differential heat flow (DSC) and mass loss (TG) of bastnaesite samples in the temperature range from room temperature to 1000 °C with a heating speed of 10 °C min−1 under air atmosphere. S-3400N scanning electron microscope (SEM) (Hitachi) was utilized to detect the surface morphology of the product. PXSJ-216 ion meter connected with a fluoride ion selective electrode and saturated calomel electrode (Shanghai Precision & Scientific Instrument Co., Ltd.) was utilized to detect the concentration of fluoride.

2.2 Experimental processes

Firstly, 10 g of bastnaesite concentrate was mixed with a certain amount of aluminum hydroxide homogeneously in a porcelain boat, and then the mixed minerals were put into a muffle furnace and calcined for a predetermined temperature and time. Secondly, the calcined ore was leached by sulfuric acid at the liquid–solid mass ratio of 10 with stirring and heating for a certain period of time. After filtered, the leaching liquid and residue were obtained. The leaching residue was washed several times with deionized water, and dried in an oven at 100 °C, then ground for detection. Thirdly, the HDEHP diluted with kerosene to the required concentration was used as extractant. The extraction of rare earths was performed by mixing equal volumes of leaching liquid and extractant in a separating funnel for 20 min by a mechanical stirrer. After two-phase separation, the raffinate was analyzed. Finally, the raffinate containing aluminum fluoride complexes was used to recover fluorine by producing cryolite. The sodium fluoride was added to adjust the F/Al and Na/Al molar ratios, and the sodium hydroxide or ammonia was used to adjust the pH. After precipitation, the cryolite product was filtered and washed several times with deionized water, then dried for 3 h at 100 °C. The supernatant solution was analyzed.

2.3 Analyses

The contents of related elements in the bastnaesite or leaching residue samples were analyzed by XRF method. The concentration of Ce4+ was determined by titration with standard (NH4)2Fe(SO4)2 solution using sodium diphenylamine sulfonate as indicator. The concentration of RE3+ was determined by titration with standard EDTA solution using xylenol orange as indicator. The concentration of Al3+ was determined by EDTA reverse titration with standard zinc solution using xylenol orange as indicator. The concentration of F was determined by fluoride ion selective electrode, and the ionic strength and the pH were maintained with total ionic strength adjusting buffer (TISAB).

The leaching rates of F, Ce and total RE were calculated as following formula:

 
image file: c6ra28106k-t1.tif(1)
where ηi is the leaching rates of F, Ce and total RE, %; Ci is the concentration of various elements in the leaching solution, g L−1; V is the volume of the leaching solution, L; m is the mass of bastnaesite concentrate, g; wi is the content of various elements in bastnaesite concentrate, %.

3 Results and discussion

3.1 TG-DSC and XRD analyses of bastnaesite

In order to study the decomposition process of bastnaesite concentrate calcined with aluminum hydroxide and the decomposition temperature range, the TG-DSC analysis was carried out, and the results are shown in Fig. 1. As shown in Fig. 1(a), the endothermic peak appeared in the range of 420–510 °C could be attributed to the decomposition of bastnaesite, and the mass loss was due to the release of CO2. There were two endothermic peaks on the TG-DSC curves of mixed ores added with aluminum hydroxide in the temperature ranges of 225–300 °C and 420–520 °C, respectively. The endothermic peak around 225–300 °C could be attributed to the dehydration of aluminum hydroxide, and the endothermic peak around 420–520 °C was for the decomposition of bastnaesite.
image file: c6ra28106k-f1.tif
Fig. 1 TG-DSC curves of bastnaesite samples in the air.

In order to study the decomposition reactions in calcination process, calcined ore obtained was analyzed by XRD, and the patterns are presented in Fig. 2. As shown in Fig. 2, the main phase in the bastnaesite concentrate was RECO3F and CaF2. After calcined in the air, the peaks of RECO3F mostly disappeared, indicating that the bastnaesite decomposed completely. The calcined ore without aluminum hydroxide mainly contained REOF, CeO1.66 and Ce7O12, but the calcined ore with aluminum hydroxide mainly contained REOF, RE2O3, CeO1.66, Ce7O12, and the new phase of AlF3. The Ce3+ could be oxidized to Ce4+ in the calcination process; however, the oxygen content in calcination atmosphere was not enough to oxidize Ce2O3 to CeO2 completely, resulting in the formation of the mixed-valent cerium oxides CeO1.66 and Ce7O12.21–23 Aluminum hydroxide began to dehydrate at the temperature above 225 °C, and transformed into activated aluminum oxide which could capture fluoride in REOF.24 The appearance of RE2O3 and AlF3 implied that Al2O3 reacted with REOF, and the fluorine was fixed by forming AlF3 rather than discharged into the environment. Combining TG-DSC and XRD analyses, the main reactions are inferred as follows:22

 
2Al(OH)3 → Al2O3 + 3H2O↑ (2)
 
3REFCO3 → REF3 + RE2O3 + 3CO2 (3)
 
REF3 + RE2O3 → 3REOF (4)
 
3CeOF + 1/2O2 → 2CeO2·CeF3 (5)
 
Ce2O3 + 0.16O2 → 2CeO1.66 (6)
 
14Ce2O3 + 3O2 → 4Ce7O12 (7)
 
6REOF + Al2O3 → 2AlF3 + 3RE2O3 (8)


image file: c6ra28106k-f2.tif
Fig. 2 XRD patterns of bastnaesite concentrate before and after calcination (calcination temperature 500 °C and calcination time 1 h).

3.2 Leaching of fluorine and REs

3.2.1 Mechanism of leaching process. Leaching residues of calcined bastnaesite concentrate with and without aluminum hydroxide were also analyzed by XRD, and the patterns are performed in Fig. 3. It is demonstrated that the leaching residue without aluminum hydroxide mainly contained BaSO4, SrSO4, CaSO4, REF3, CaF2 and SiO2, while the leaching residue with aluminum hydroxide mainly contained BaSO4, SrSO4, CaSO4 and SiO2. The main chemical compositions of leaching residues of calcined bastnaesite concentrate with and without aluminum hydroxide are listed in Tables 3 and 4. It indicates that the adding of aluminum hydroxide could greatly promote the leaching of insoluble fluorides and REs. The unreacted Al2O3 could ionize out Al3+ ions in sulfuric acid condition. Due to the hard–hard combination of the soft–hard acid base (SHAB) concept, the Al3+ ions have good affinity with F anions to form [AlFn](3−n) complex ions,25,26 which will promote the dissolution of CaF2 and REF3, and thus reduce the discharge of fluorine-containing waste. The most possible reactions during the process can be provided as follows:
 
Al2O3 + 6H+ → 2Al3+ + 3H2O (9)
 
nREOF + RE2O3 + CeO2 + (2n + 10)H+ + Al3+ = [AlFn](3−n) + Ce4+ + (n + 2)RE3+ + (n + 5)H2O (10)
 
nCaF2 + 2Al3+ + nH2SO4 → 2[AlFn](3−n) + nCaSO4↓ + 2nH+ (11)
 
nREF3 + 3Al3+ → 3[AlFn](3−n) + nRE3+ (12)
 
AlF3 + Al3+ → AlF2+ + AlF2+ (13)

image file: c6ra28106k-f3.tif
Fig. 3 XRD patterns of leaching residues (sulfuric acid concentration 3 mol L−1, leaching temperature 90 °C and leaching time 1 h).
Table 3 The main chemical composition of the leaching residue of calcined bastnaesite concentrate (wt%)
Component SrO SO3 BaO CaO F RExOy SiO2
Content/% 18.82 18.41 15.50 13.63 12.17 8.71 2.52


Table 4 The main chemical composition of the leaching residue of calcined bastnaesite concentrate with aluminum hydroxide (wt%)
Component SrO SO3 CaO BaO SiO2 F RExOy
Content/% 25.74 24.75 17.86 13.59 3.45 0.51


3.2.2 Effect of n(Al)/n(F). The effect of n(Al)/n(F) on the leaching rates of fluorine and REs is shown in Fig. 4. It can be seen that the leaching rates of F, Ce and total RE were around 65.32%, 90.34% and 90.57% of calcined bastnaesite without additive. When the n(Al)/n(F) was 1/6, the leaching rates of F, Ce and total RE significantly increased to 87.04%, 98.65% and 97.42%. This is because that the defluorination reaction of REOF will accelerate the decomposition of REFCO3. Further increase in n(Al)/n(F), the changes of leaching rates of Ce and total RE were not obvious but the leaching rate of F continued to increase. The leaching rate of F reached 93% at the n(Al)/n(F) of 1/2. Therefore, the additive amount of Al(OH)3 is selected as n(Al)/n(F) of 1/2.
image file: c6ra28106k-f4.tif
Fig. 4 Effect of n(Al)/n(F) on leaching rates of fluorine and REs (calcination temperature 500 °C, calcination time 1 h, sulfuric acid concentration 3 mol L−1, leaching temperature 90 °C and leaching time 1 h).
3.2.3 Effect of calcination temperature. The bastnaesite decomposes in the range of 425–560 °C.27 It is necessary to control the appropriate reaction temperature. The effect of calcination temperature was examined as shown in Fig. 5. It is found that the leaching rates increased fast in the range of 400–500 °C. Continue raising the temperature, the leaching rates of Ce and total RE had a little decrease when the temperature higher than 600 °C. This is because that when the calcination temperature lower than 500 °C, the bastnaesite decomposes incompletely, resulting in the low leaching rates of fluorine and REs; when the calcination temperature higher than 600 °C, the rare earth oxides have crystal transformation phenomenon which will decrease the activity of bastnaesite,28 leading to the lower leaching rate of REs. According to the results, the appropriate reaction temperature is 500–600 °C. Taking into account the energy efficiency, a calcination temperature of 500 °C is selected.
image file: c6ra28106k-f5.tif
Fig. 5 Effect of calcination temperature on leaching rates of fluorine and REs (n(Al)/n(F) 1/2, calcination time 1 h, sulfuric acid concentration 3 mol L−1, leaching temperature 90 °C and leaching time 1 h).
3.2.4 Effect of calcination time. The effect of calcination time on the leaching rates of fluorine and REs is shown in Fig. 6. The results show that the leaching rates of fluorine and REs remarkably increased with the increase of calcination time and reached the maximum values at 1 h, at which the leaching rates of F, Ce and total RE were 92.71%, 98.92% and 98.61%. However, the leaching rates had a little decline when the calcination time was longer than 2 h, which may be due to the generation of more insoluble fluosilicate.29 Therefore, a calcination time of 1 h can be selected.
image file: c6ra28106k-f6.tif
Fig. 6 Effect of calcination time on leaching rates of fluorine and REs (n(Al)/n(F) 1/2, calcination temperature 500 °C, sulfuric acid concentration 3 mol L−1, leaching temperature 90 °C and leaching time 1 h).
3.2.5 Effect of sulfuric acid concentration. The effect of sulfuric acid concentration on the leaching rates of fluorine and REs is shown in Fig. 7. It is seen from Fig. 7 that both the leaching rates of F, Ce and total RE increased with the increase in sulfuric acid concentration, and had no beneficial effect with acid concentration higher than 3 mol L−1. Excessively low acidity in the leaching solution can not react with calcined ore thoroughly, leading to the low leaching rates of fluorine and REs. However, excessively high acidity in the leaching solution is unfavorable for the subsequent extraction process.1 Therefore, a concentration of 3 mol L−1 is selected as the optimum acidity of leaching solution.
image file: c6ra28106k-f7.tif
Fig. 7 Effect of sulfuric acid concentration on leaching rates of fluorine and REs (n(Al)/n(F) 1/2, calcination temperature 500 °C, calcination time 1 h, leaching temperature 90 °C and leaching time 1 h).
3.2.6 Effect of leaching temperature. The effect of leaching temperature on the leaching rates of fluorine and REs is shown in Fig. 8. The results showed that the higher the temperature was, the higher the leaching rates of F, Ce and total RE were. The leaching rate of F was promoted from 78.58% to 92.00% with the temperature increased from 60 °C to 90 °C while the leaching rates of Ce and total RE only increased quickly with the temperature higher than 75 °C, and both had no obvious rising when the leaching temperature was over 90 °C. Therefore, a leaching temperature of 90 °C is chosen as the optimal temperature for the leaching experiments.
image file: c6ra28106k-f8.tif
Fig. 8 Effect of leaching temperature on leaching rates of fluorine and REs (n(Al)/n(F) 1/2, calcination temperature 500 °C, calcination time 1 h, sulfuric acid concentration 3 mol L−1 and leaching time 1 h).
3.2.7 Effect of leaching time. The effect of leaching time on the leaching rates of fluorine and REs is shown in Fig. 9. It is found from Fig. 9 that the leaching rates of Ce and total RE were nearly 98% at 0.5 h and had no obvious increase with the prolonging of leaching time. However, the leaching rate of F increased significantly with the reaction. The difference in the leaching speed of fluorine and REs proves that the fluorine is not leached out entirely with rare earths. The leaching rate of F could be above 90% after leaching for 1 h.
image file: c6ra28106k-f9.tif
Fig. 9 Effect of leaching time on leaching rates of fluorine and REs (n(Al)/n(F) 1/2, calcination temperature 500 °C, calcination time 1 h, sulfuric acid concentration 3 mol L−1 and leaching temperature 90 °C).

3.3 Separation of fluorine and REs

The obtained sulfuric acid leaching solution contained 0.58 mol L−1 F, 0.30 mol L−1 Al3+, 0.28 mol L−1 Ce4+, 0.21 mol L−1 RE3+, 1.50 mol L−1 H+, etc. The Ce4+ was extracted by mixing equal volumes of leaching solution and 1 mol L−1 HDEHP, then the Ce4+-absence solution was obtained. The RE3+ concentrate was extracted by mixing equal volumes of HDEHP and the resulting Ce4+-absence solution which had been adjusted to pH 3.8 by ammonia. The results are presented in Table 5. It is found that after three times of extraction, the Ce4+ and RE3+ were extracted into organic phase and almost all of the F and Al3+ were left in raffinate. This is because that fluoride and aluminum mainly exist as [AlFn](3−n) complex in acidic solution,26 and the [AlFn](3−n) complex cannot be extracted by HDEHP, which is leading to the separation of fluorine and REs.
Table 5 Concentrations of F, Al3+, Ce4+ and RE3+ in leaching solution
Extraction times [F] (mol L−1) [Al3+] (mol L−1) [Ce4+] (mol L−1) [RE3+] (mol L−1)
0 0.58 0.30 0.28 0.21
1 0.56 0.30 0.02 0.21
2 0.56 0.29 0.08
3 0.56 0.29


3.4 Recovery of fluorine

The raffinate containing 0.56 mol L−1 F and 0.29 mol L−1 Al3+ which mainly exist as aluminum fluoride complexes [AlFn](3−n) was used to produce cryolite so as to recover the fluorine resource in bastnaesite. It is known that the ratio of F/Al in aluminum fluoride complex [AlFn](3−n) greatly depends on the contents of fluoride and aluminum. In order to recover the fluoride and aluminum in the raffinate as much as possible, the sodium fluoride was added to adjust the F/Al and Na/Al molar ratios, and the sodium hydroxide or ammonia was added to adjust the pH to around 4.5–5.0. The reaction temperature was controlled within 80–90 °C. The solubility of Na3AlF6 is 4 × 10−10,30 making it easy to precipitate from solution. Fig. 10 shows the XRD pattern of the product. The characteristic peaks of Na3AlF6 were observed and the prepared product was found to be monoclinic phase cryolite. Fig. 11 gives the SEM image of the product. It is found that the obtained cryolite consisted of even and uniform granules with an average diameter of 1–2 μm. The results in Table 6 showed that the high recovery rates of fluoride and aluminum greater than 96% could be obtained, indicating that the preparation of cryolite is an effective method to recover fluorine resource in bastnaesite.
 
[AlFn](3−n) + (6 − n)F → AlF63− (14)
 
3Na+ + AlF63− → Na3AlF6 (15)

image file: c6ra28106k-f10.tif
Fig. 10 XRD pattern of the prepared cryolite.

image file: c6ra28106k-f11.tif
Fig. 11 SEM photograph of the prepared cryolite.
Table 6 Recovery rates of fluoride and aluminum
  Fluoride Aluminum
[F] and [Al3+] of raffinate/(mol L−1) 0.56 0.29
Volume of raffinate/(L) 0.10 0.10
Amount of supplemental sodium fluoride/(mmol) 45.0
[F] and [Al3+] of supernatant solution/(mmol L−1) 37.1 7.60
Volume of supernatant solution/(L) 0.10 0.10
Recovery rate/(%) 96.33 97.38


4 Conclusions

In order to solve the problems of fluorine loss and contamination, and recover the fluorine resource in bastnaesite, a new clean process of decomposing bastnaesite with aluminum hydroxide followed by sulfuric acid leaching was proposed. In the oxidation calcination process, fluorine could be taken up by Al2O3, preventing the discharge of fluorine. After calcination, leaching for calcined ore was performed with dilute sulfuric acid. Aluminum could promote the dissolution of CaF2 and REF3 in bastnaesite. The optimum conditions were determined as n(Al)/n(F) 1/2, calcination temperature 500 °C, calcination time 1 h, sulfuric acid concentration 3 mol L−1, leaching temperature 90 °C and leaching time 1 h, at which the leaching rates of F, Ce and total RE reached 92.71%, 98.92% and 98.61%. Fluorine could be separated from REs after extraction process, and was recovered as Na3AlF6 with the recovery rates of fluoride and aluminum greater than 96%. This technology has an important practical significance to further develop rare earth metallurgical industry and protect environment.

Acknowledgements

The financial aids from the key program of National Natural Science Foundation of China (NSFC: 50934004), National Natural Science Foundation of China (51274061), Major State Basic Research Development Program of China (973 Program: 2012CBA01205) and Fundamental Research Supporting Project of Northeastern University (N110602006) are gratefully acknowledged.

References

  1. W. Y. Wu, Rare Earth Metallurgy, Chemical Industry Press, Beijing, 2005, p. 56 Search PubMed.
  2. Y. Kanazawa and M. Kamitani, J. Alloys Compd., 2006, 408–412, 1339–1343 CrossRef CAS.
  3. W. P. Liu, X. M. Wang, Z. X. Wang and J. D. Miller, Miner. Eng., 2016, 85, 17–22 CrossRef CAS.
  4. S. C. Sun, Z. Y. Wu, B. Gao, X. Bian, W. Y. Wu and G. F. Tu, J. Rare Earths, 2007, 25(4), 508–511 CrossRef.
  5. X. W. Huang, Z. Q. Long, H. W. Li, W. J. Ying, G. C. Zhang and X. X. Xue, J. Rare Earths, 2005, 23(1), 1–4 Search PubMed.
  6. G. C. Zhu, J. Tian, R. A. Chi and S. M. Xu, Chemistry, 2000, 63(12), 6–11 Search PubMed.
  7. Q. W. Zhang and F. Saito, Hydrometallurgy, 1998, 47(2), 231–241 CrossRef CAS.
  8. Y. Abdulkerim, O. Abdullah and G. Ismail, Hydrometallurgy, 2003, 68(1–3), 195–202 Search PubMed.
  9. S. L. Zhao, C. G. He, Z. J. Cao, Y. Liu and F. Zhao, Chin. Rare Earths, 2003, 24(4), 32–35 Search PubMed.
  10. Y. K. Huang, T. A. Zhang, Z. H. Dou, J. Liu and F. F. Tang, J. Rare Earths, 2014, 32(11), 1043–1047 CrossRef CAS.
  11. T. Xu and H. Q. Peng, J. Rare Earths, 2009, 27(6), 1096–1102 CrossRef.
  12. A. Bhatnagara, E. Kumara and M. Sillanpää, Chem. Eng. J., 2011, 171(3), 811–840 CrossRef.
  13. J. Qiao, C. R. Zhang, S. G. Liu and X. K. Hao, Chin. Rare Earths, 1997, 18(3), 64–67 Search PubMed.
  14. R. M. Sawant, R. K. Rastogi, M. A. Mahajan and N. K. Chaudhuri, Talanta, 1996, 43(1), 89–94 CrossRef CAS PubMed.
  15. Z. F. Zhang, F. Q. Guo, S. L. Meng, Q. Jia, H. F. Li and D. Q. Li, Ind. Eng. Chem. Res., 2010, 49, 6184–6188 CrossRef CAS.
  16. G. C. Zhu, J. Tian, R. A. Chi, S. M. Xu and Z. G. Zhang, Chin. Rare Earths, 2001, 22(3), 30–33 Search PubMed.
  17. Z. G. Liu, Q. S. Yang, L. S. Liu, S. S. Guo, B. Z. Chen, X. J. Wei and A. N. Hu, Chin. Rare Earths, 2004, 25(2), 20–25 Search PubMed.
  18. L. S. Wang, C. M. Wang, Y. Yu, X. W. Huang, Z. Q. Long, Y. K. Hou and D. L. Cui, J. Hazard. Mater., 2012, 209–210(4), 77–83 CrossRef CAS PubMed.
  19. H. Y. Fu, Y. Y. Wei, Y. Li and J. G. He, J. Chin. Soc. Rare Earths, 2013, 31(4), 393–398 CAS.
  20. Z. Akdeniz, Z. Cicek and M. P. Tosi, Chem. Phys. Lett., 1999, 308(5–6), 479–485 CrossRef CAS.
  21. E. A. Kümmerle and G. Heger, J. Solid State Chem., 1999, 147(2), 485–500 CrossRef.
  22. Y. Yang, S. C. Sun, X. P. Zhu, W. Jia and G. F. Tu, J. Chin. Soc. Rare Earths, 2015, 33(1), 95–100 CAS.
  23. M. Zinkevich, D. Djurovic and F. Aldinger, Solid State Ionics, 2006, 177(177), 989–1001 CrossRef CAS.
  24. Z. H. Peng, Q. F. Li and Q. S. Zhou, Light Metals, 2010, 5, 16–18 Search PubMed.
  25. B. R. Martin, Coord. Chem. Rev., 1996, 149(1), 23–32 CrossRef.
  26. B. J. Plankey and H. H. Patterson, Environ. Sci. Technol., 1986, 20(2), 160–165 CrossRef CAS PubMed.
  27. W. Y. Wu, X. Bian, Z. Y. Wu, S. C. Sun and G. F. Tu, Trans. Nonferrous Met. Soc. China, 2007, 17(4), 864–868 CrossRef CAS.
  28. M. H. Wang, M. Zeng, L. S. Wang, J. H. Zhou, D. L. Cui, Q. G. Wang, R. G. Weng and X. S. Chen, J. Chin. Soc. Rare Earths, 2013, 31(2), 148–153 CAS.
  29. J. Zhou, C. H. Yan and C. S. Liao, Chin. Rare Earths, 1998, 19(3), 9–17 Search PubMed.
  30. M. Kumar, M. N. Babu, T. R. Mankhand and B. D. Pandey, Hydrometallurgy, 2010, 104(2), 304–307 CrossRef CAS.

This journal is © The Royal Society of Chemistry 2017
Click here to see how this site uses Cookies. View our privacy policy here.