Yi-Zu Liua,
Karthikeyan Manivannana,
Ai-Wei Leeb,
Yan-Jiun Huangc,
Po-Li Weid and
Jem-Kun Chen*a
aDepartment of Materials Science and Engineering, National Taiwan University of Science and Technology, 43, Sec 4, Keelung Rd, Taipei, 106, Taiwan, Republic of China. E-mail: jkchen@mail.ntust.edu.tw; Fax: +886-2-27376544; Tel: +886-2-27376523
bDepartment of Anatomy and Cell Biology, School of Medicine, College of Medicine, Taipei Medical University, Taipei 110, Taiwan
cDepartment of Surgery, College of Medicine, Division of Colorectal Surgery, Taipei Medical University Hospital, Taipei Medical University, The PhD Program for Translational Medicine, College of Science and Technology, Academia Sinica, Taipei, Taiwan
dCancer Center, Division of General Surgery, Department of Surgery, Taipei Medical University Hospital, College of Medicine, Graduate Institute of Cancer Biology and Drug Discovery, Taipei Medical University, Taipei, Taiwan
First published on 26th April 2017
We grafted azido-terminated poly(N-isopropylacrylamide) (PNIPAAm) brushes onto thin gold films on silicon as a bottom electrode. A probe of single-stranded DNA (ssDNA) presenting a 4-pentynoic acid succinimidyl ester unit was grafted onto the azido-terminated PNIPAAm brushes through a click reaction, resulting in block copolymer brushes. The PNIPAAm-b-ssDNA copolymer brushes formed homogeneous complexes stabilized via bio-multiple hydrogen bonds (BMHBs), which enhanced proton transfer and thereby decreased the resistivity of the structures. The homogeneous complex state of the PNIPAAm-b-ssDNA copolymer brushes transformed into a phase-separated state after hybridization with 0.5 pg nL−1 of its target DNA, which resulted from competition between the BMHBs and complementary HBs; this phase transformation of the PNIPAAm and probe segments inhibited proton transfer and significantly increased the resistivity. Furthermore, hybridization with mismatched DNA sequences generated sufficient “proton leakage” to decrease the resistivity at temperatures below the lower critical solution temperature (LCST), especially for adenine and guanine units. Sequences with thymine and cytosine mismatches could be distinguished from the target at temperatures above the LCST due to disruption of the BMHBs at increased temperatures (80 °C). The ability to detect label-free DNA and recognize sequence mismatches suggests the potential use of these novel materials in bioelectronics.
In recent years, DNA microarrays have been used on surface-immobilized single-stranded DNA (ssDNA) probes, which has aided their flexibility and enabled considerable data generation.10 However, the fluorescent emission of labelled target DNA cannot be detected by conventional methods. Hence, label-free methods are useful for supporting quantitative detection of DNA binding, scalability, and multiplexing, as well as the expense of the operation.11 Herein, for the first time, we report a label-free technique for DNA detection. DNA block copolymers are a new emerging class of functional hybrid polymers composed of an oligonucleotide strand covalently attached to another polymer. Based on their amphiphilicity and molecular recognition properties,12 DNA block copolymers can be assembled into various types of nanostructures, which are useful for several applications, ranging from DNA-templated syntheses13 to gene therapy14 and drug delivery.15 For example, Mirkin and coworkers showed that spherical micelles of DNA-block-polystyrene (DNA-b-PS) can be assembled into macroscopic polymer networks showing cooperative sharp melting transitions.16 The simultaneous self-assembly of DNA-b-PS and magnetic nanoparticles is used to fabricate nanoparticle-loaded DNA block copolymer assemblies. This process can dramatically enhance DNA-binding properties.17 Researchers have also shown that DNA block copolymers can be assembled into various morphologies by utilizing the molecular recognition property of DNA.18,19 Gianneschi and co-workers synthesized a DNA brush copolymer that undergoes a reversible sphere-to-cylinder morphology change by DNA cleavage and hybridization.20 Herrmann et al. reported the formation of rodlike assemblies of DNA-block-poly(propylene oxide) (DNA-b-PPO) using a long repetitive complementary DNA strand as a template.21 The rod-shaped aggregates showed significantly higher cellular uptake than spheres,22 demonstrating that the ability to control the morphology of DNA assemblies is important for their biological and medical applications.23–25
Alemdaroglu et al. observed the strength of the bio-multiple hydrogen bonds (BMHBs) in poly(N-isopropylacrylamide) (PNIPAAm) and nucleobases to follow the sequence guanine (G) > adenine (A) > thymine (T) > cytosine (C) > uracil (U). The presence of BMHBs can enhance the degree of H+ transport in a PNIPAAm film, which is caused by a notable change in electronic conductivity. The insulator PNIPAAm can be altered into a semiconducting form via a simple method.13 In the present study, we formed novel DNA recognition layers, with PNIPAAm-b-ssDNA copolymer brushes acting as aptamers, that changed conductivity upon homogeneous complexation and phase separation of the PNIPAAm and ssDNA segments. Copolymer brushes can change structure in situ on the surface during hybridization. PNIPAAm and ssDNA, which are regarded as an insulator and conductor, respectively, are miscible due to BMHBs. Our target was the DNA strand complementary to the ssDNA segment of the copolymer brushes.26 Upon grafting polymerization with ssDNA, homogeneous complexes were generated to facilitate proton transport in the films, leading to a decline in resistance. Because the HB between the target and probe (ssDNA) was much stronger than the BMHBs between the PNIPAAm and ssDNA segments, hybridization of the target with the PNIPAAm-b-ssDNA copolymer brushes changed the morphology significantly. The probe segments preferred to release from the complex and bond to the target. The isolated PNIPAAm segments blocked proton transport from the bottom to the top electrodes, resulting in an increase in resistance (Scheme 1). We examined the selectivity and sensitivity of the complexation/decomplexation of PNIPAM-b-ssDNA copolymer brushes by subjecting them to a target featuring single-nucleic-acid mismatches at various temperatures. The developed aptamers are potentially applicable for DNA recognition sensors.
Scheme 1 Homogeneous complexation, stabilized through BMHBs, and phase separation of PNIPAAm and ssDNA segments after hybridization with the target. |
The substitution reaction was carried out overnight by exposing the bromo-terminated substrates to a saturated solution of NaN3 in DMF in a covered container. Then, the sample was rinsed with DMF followed by methanol and deionized water before drying in a N2 stream. After these reactions, the wafers were placed in a Soxhlet apparatus to remove non-grafted materials and then dried under N2 prior to use. A solution of 4-pentynoic acid succinimidyl ester-conjugated probe (100 nmol) in 2.5 mL phosphate buffer (PB) (pH 7.2, 20 mM) and 1 × 1 cm2 grafted azido-PNIPAAm samples were added to a 10 mL plastic culture tube. A stock solution (0.1 mL) of catalyst/ligand (1.0 mmol of CuSO4, 1.1 mmol of TBTA) in dimethyl sulfoxide (DMSO)/water (v/v, 1/1) and 4.0 mmol (0.79 mg) of sodium ascorbate were then added. The reaction mixture was agitated for 20 h at 15 °C. The as-prepared samples were incubated overnight at room temperature in the solution and then washed thrice with washing buffer [10 mM Tris–HCl (pH 7.5), 150 mM NaCl, 0.05% Tween 20] and thrice with water. The samples were blow-dried under N2 to ensure that their surfaces were dry and free of dust particles. In addition, ssDNA was grafted to an azido-modified Au substrate without PNIPAAm in a blank experiment to analyze the thickness.
Herein, the surfaces presenting PNIPAAm that had been grafted for 4, 8, 12, 16, and 20 h were denoted PN4, PN8, PN12, PN16, and PN20, respectively, and sequentially grafted with ssDNA to form aptamers of PNIPAAm-b-ssDNA copolymer brushes, which were denoted PN4D, PN8D, PN12D, PN16D, and PN20D, respectively. The label-free target, AM, TM, GM, and CM were diluted with a hybridization buffer [comprising SSC (3 M NaCl, 0.3 M sodium citrate·2H2O, pH 7), Denhardt's solution (1% bovine serum albumin), 2% Ficoll400, 2% polyvinylpyrollidone, and 0.5% sodium dodecyl sulfate] to a final concentration of 50 μM. Two small strips of adhesive tape were affixed along the rim of the substrate and then covered with a clean microscope slide cover glass. The cavity formed between the chip and cover glass was filled by slowly loading the hybridization solution (≈30 μL) under capillary force. After removal of the cover glass, the chip was washed thrice with washing buffer and then with copious amounts of water and blow-dried under N2. Control experiments were performed in the same manner using AM, TM, GM, and CM, which had lengths similar to that of the target but only partial complementarity. Water contact angles of PNIPAAm-b-ssDNA copolymer brushes were measured after they had been dried under a flow of N2. The chemical compositions of the modified silicon surfaces were determined through X-ray photoelectron spectrometry (XPS; Scientific Theta Probe, UK).33 The thicknesses of the copolymer grafts on the silicon substrates were measured using ellipsometry (SE-5; Sopra, France). The tethered copolymer brushes were stripped from the surface through immersion in HF solution (5 wt%) for 5 min at room temperature. The stripped copolymers were analyzed using gel permeation chromatography after purification through extensive dialysis against deionized water, which was performed using a VISCOTEK-DM400 instrument equipped with a LR 40 refractive index detector. Monodisperse polymer standards (Polymer Lab; Agilent Technologies, USA) were used to generate a calibration curve.
The electroactivities of the PNIPAAm-b-ssDNA copolymer brushes were studied by I–V curve measurements. That is, platinum (Pt) electrodes (thickness: 200 nm) were coated onto the sample surfaces via stainless-steel shadow masks as the top electrode. Then, the samples were lyophilized 24 h prior to use of I–V curves from the top to the bottom electrode of the Au substrate (Scheme 2). All the measurements were performed at room temperature with a relative humidity of 35–45%. Repeated measurements were within 5% of the average value for each sample. To prevent metal contamination, the interval between the Pt electrodes was ≈6.5 mm. The resistivity of each copolymer film was measured at 25 and 80 °C; voltage sweeps were recorded in the range from −0.2 to +0.2 V.
Scheme 2 Schematic representation of the structured device used to measure the resistivities of PNIPAAm-b-ssDNA copolymer brushes. |
Fig. 2 (a) O/C, (b) N/C and (c) P/C atomic ratios of the PNIPAAm-b-DNA copolymer brushes at 25, 45 and 80 °C. |
The brush parameters of the dry PNIPAAm-b-ssDNA brushes were estimated by the ellipsometric dry layer thickness (h),37 PNIPAAm and ssDNA bulk density of 1.1 and 1.7 g cm−3, respectively. These calculations were made with their roughnesses (Ra), grafting densities (σ), distance between grafting sites (dg), molecular weight, and surface coverage (Sc). Furthermore, we examined the temperature-sensitive activities of these PNIPAAm-b-ssDNA films in contact with aqueous solutions using the SWCA measurements. Table 1 presents the calculated data of layer parameters for ssDNA, PNIPAAm, and PNIPSSm-b-ssDNA films. The layer parameters (molecular weights (Mn and Mw), Sc, dg, and σ) increased gradually with low polydispersity index (PDI) values upon increasing the polymerization times for tethered PNIPAAm films. Slight increases in these layer parameter were obtained after ssDNA immobilization at the chain end. The thicknesses of the PNIPAAm-b-ssDNA layers decreased slightly with increasing temperature from 25 to 45 °C because the intramolecular HBs among PNIPAAm groups was stronger than the BMHBs between the PNIPAAm and ssDNA segments. In addition, the SWCAs of PN4D, PN8D, PN12D, PN16D, and PN20D brushes exhibited thermally responsive switching between hydrophilic and hydrophobic states at temperatures below and above the LCST, respectively. The SWCAs of the PN4D brushes were 78.5 and 46.9° at 25 and 45 °C, respectively. This thermal responsivity of PN4D was completely opposite to that of pure PNIPAAm (Table 1), which can be explained by considering the miscibility of the PNIPAAm and ssDNA segments at 25 °C. The HB interactions between the PNIPAAm and ssDNA segments resulted in the hydrophilic groups residing within these molecules, thereby exposing the hydrophobic groups on the surface at 25 °C. The HB interactions between the PNIPAAm and ssDNA segments weakened significantly at 45 °C. This was due to the predominance of intramolecular HBs of the PNIPAAm segments,38 which drove the ssDNA segments to the surface, leading to a hydrophilic surface state. Upon increasing the thickness of the PNIPAAm segment, the SWCA at 25 °C decreased from 78.5° for PN4D to 64.5° for PN8D, whereas the SWCA at 45 °C increased from 46.9 to 51.7°. The SWCAs of PN12D at 25 and 45 °C were 49.8 and 56.3°, respectively. These observations showed that PNIPAAm-b-ssDNA exhibited minimal thermoresponsive behavior. Notably, the thermoresponsive behavior of the copolymer brushes became similar to that of tethered PNIPAAm films when grafting of the PNIPAAm segment had been performed for >12 h (Table 1). The difference in the SWCAs between the hydrophilic (34°) and hydrophobic (62.1°) states reached 28.1° for PN16D. For PN20D, the thermal responsive behavior was close to that of pure PNIPAAm brushes. Our results indicate that when its thickness was >300 nm, the PNIPAAm segment predominated the surface properties.
Samples | Mn/1000 (g mol−1) | Mw/1000 (g mol−1) | PDI (Mw/Mn) | Tga (°C) | Scb (mg m−2) | dgc (nm) | σd (nm−2) | he (nm) | Raf (nm) | SWCA (degree) | |||
---|---|---|---|---|---|---|---|---|---|---|---|---|---|
25 °C | 45 °C | 25 °C | 45 °C | 25 °C | 45 °C | ||||||||
a Tg was obtained from DSC data (Fig. S2).b Sc = ρh.c d σ = dg−2.e Thickness (h) was obtained from ellipsometry.f Roughness (Ra) was obtained from AFM. | |||||||||||||
ssDNA | 6.2 | 6.7 | 1.08 | — | 8.3 | 0.35 | 8.03 | 75.4 | 75.4 | 2.6 | 2.5 | 23.5 ± 3 | 22.1 ± 4 |
PN4 | 11.1 | 14.9 | 1.34 | 133.6 | 14.5 | 0.36 | 7.84 | 131.9 | 86 | 9.3 | 7.5 | 34.6 ± 4 | 79.7 ± 4 |
PN8 | 32.3 | 40.1 | 1.24 | 134.2 | 22.4 | 0.49 | 4.16 | 203.6 | 135 | 8.4 | 6.7 | 35.9 ± 4 | 84.3 ± 4 |
PN12 | 57.4 | 67.3 | 1.17 | 134.3 | 32.9 | 0.54 | 3.44 | 299.1 | 202 | 7.8 | 6.1 | 32.5 ± 3 | 85.8 ± 4 |
PN16 | 75.6 | 87.7 | 1.16 | 134.8 | 38.8 | 0.57 | 3.08 | 352.4 | 241 | 7.2 | 5.8 | 33.6 ± 3 | 86.4 ± 3 |
PN20 | 100.7 | 116.2 | 1.15 | 134.9 | 46.9 | 0.60 | 2.80 | 426.6 | 298 | 6.9 | 5.3 | 31.1 ± 3 | 86.5 ± 3 |
PN4D | 17.3 | 21.1 | 1.22 | 103.3 | 14.5 | 0.45 | 5.04 | 132.1 | 97.3 | 5.2 | 3.6 | 78.5 ± 4 | 46.9 ± 4 |
PN8D | 38.5 | 46.3 | 1.20 | 110.1 | 22.4 | 0.54 | 3.49 | 203.8 | 145.8 | 4.8 | 3.5 | 64.5 ± 4 | 51.7 ± 4 |
PN12D | 63.6 | 73.5 | 1.16 | 116.5 | 32.9 | 0.57 | 3.11 | 299.3 | 212.5 | 4.2 | 3.4 | 49.8 ± 3 | 64.3 ± 4 |
PN16D | 81.8 | 93.9 | 1.15 | 121.4 | 38.8 | 0.59 | 2.84 | 352.6 | 251.4 | 3.9 | 3.2 | 34.2 ± 3 | 77.1 ± 3 |
PN20D | 106.9 | 122.4 | 1.14 | 124.8 | 46.9 | 0.62 | 2.64 | 426.8 | 308.3 | 3.6 | 3.2 | 32.2 ± 3 | 83.3 ± 3 |
Fig. 3 Surface SEM images of PN8D copolymer brushes (a) before and (b) after hybridization with the target. |
BMHBs can improve H+ transport in PNIPAAm-b-ssDNA copolymer brushes,18,19 so we focused mainly on determining the temperature-responsive resistance of our functionalized surfaces. The linear I–V curves exhibited ohmic behavior at 25 and 80 °C during device use (Scheme 2). The slopes of I–V curves corresponded to the resistivities of the surfaces at particular temperatures. Fig. 4 shows the logarithms of the average resistivities for PN4D, PN8D, PN12D, PN16D, and PN20D brushes at different temperatures from 20 to 90 °C. In particular, there were no I–V curves for the neat PNIPAAm film because proton transport did not occur. Therefore, we could not measure the resistivity of the neat PNIPAAm brushes, which could be regarded as an insulator. Upon grafting polymerization with ssDNA, proton transport in the films increased significantly, a result of the homogeneous complexes that were generated, leading to a decline in resistance. The resistivity of the PNIPAAm-b-ssDNA copolymer brushes increased upon increasing the thickness of the PNIPAAm segment, which is associated with the strength of BMHBs, confirming that the increases in conductivity of PNIPAAm arose from proton transport induced by BMHBs. The length ratio of ssDNA to PNIPAAm segments revealed that the improved conductivity at <30 °C occurred due to proton transport induced through BMHBs. The resistivities of the PNIPAAm-b-ssDNA copolymer brushes increased upon increasing the temperature at 70 °C, demonstrating that proton transport from the bottom to the top electrode was blocked as a result of phase separation of the PNIPAAm and ssDNA segments. The resistivities decreased abruptly from 70 to 90 °C, suggesting that increased vibrations of the PNIPAAm chains was facilitated by proton transport in the PNIPAAm-b-ssDNA copolymer brushes at >70 °C. For PN4D, PN8D and PN12D, the resistivity increased suddenly upon increasing the temperature from 30 to 40 °C due to phase separation of the PNIPAAm and ssDNA segments. The dependence of resistivity on temperature increased slowly for PN16D and PN20D, symptomatic of the fact that the effects of the increased vibration of the polymer chains at 30 to 40 °C were more evident as a result of weaker BMHBs. The resistivity transition temperature of PNIPAAm-b-ssDNA copolymer brushes were superior than the LCST because the BMHBs were improved slightly in the dry state exclusive of the association of water molecules.36 Grafting ssDNA on the PNIPAAm chains can offer increased proton transport and considerably enhanced conductivity. The ssDNA segment could be regarded as a “minority” carrier in the complexed layer, predominantly determining the resistivities of the films.39 Moreover, the variation in resistivity with temperature can be reversible for five cycles between 20 and 90 °C for all PNIPAAm-b-ssDNA copolymer brushes, indicating stable resistivity against temperature.
Fig. 4 Resistivities of the PNIPAAm-b-DNA copolymer brushes (logarithm scale) recorded with respect to temperature at 25 to 90 °C. |
Fig. 5a and b display the logarithms of the average resistivities of the PNIPAAm-b-ssDNA copolymer brushes upon hybridization with the label-free target at various concentrations at 25 and 80 °C, respectively. Notably, the resistivity might be influenced readily by the humidity or roughness of the surface. The inaccuracy ranges were marked as indices for recognition of hybridization with the target. A change in resistivity without overlapping the inaccuracy range is defined herein as a “distinguishable” value. We observed approximately linear increases in the resistivity of the grafted copolymer layer upon increasing the concentration of the target to 8 pg nL−1 at 25 °C. The resistivity reached a plateau for all samples, indicating saturation of the hybridization between the probe segment (ssDNA) and the target; the strong complementary HB resulted in phase separation of the PNIPAAm and ssDNA segments, leading to an increase in resistivity. In other words, the target could be exploited to eliminate the proton transfer of complexation at 25 °C. Interestingly, the resistivity of the copolymer brushes after hybridization with the target at 80 °C decreased linearly upon increasing the concentration, indicating that the high temperature accelerated proton transfer to overcome the barrier of phase separation. A low concentration of the minor carriers (ssDNA segments) could generate a significant change in resistivity at 80 °C. The lowest concentrations for target recognition for PN4D, PN8D, PN12D, PN16D, and PN20D brushes at 25 °C were 0.5, 0.5, 1, 2, and 4 pg nL−1, respectively; these values at 80 °C were 4, 1, 1, 0.5, and 0.5 pg nL−1, respectively. We found that the sensitivities of PN4D and PN8D for hybridization with the target were greater than those of the other samples; thus, a higher ratio of probe:PNIPAAm segments enhanced the sensitivity significantly at 25 °C. In contrast, the sensitivities of PN16D and PN20D for target detection were higher than those of the other samples at 80 °C; thus, thermal effects facilitated proton transfer of the minor carriers (ssDNA segments) within longer polymer chains at 80 °C. Furthermore, we used AM, TM, GM, and CM to investigate the ability of our surfaces to distinguish mismatched hybridization from that of the target. Fig. 6a displays the logarithms of the average resistivities of PN4D before and upon hybridization at 25 °C with the target, AM, TM, GM, and CM at a concentration of 0.5 pg nL−1. The resistivity of blank PN4D ranged from 5.69 to 6.05 Ω cm and shifted to a range from 6.09 to 6.47 Ω cm upon hybridization at 25 °C with the target. A mismatched hybridization could be regarded as resulting in “proton leakage,” leading to a decrease in resistivity. Compared with blank PN4D, the resistivity of PN4D after hybridization with AM and GM at 0.5 pg nL−1 did not change significantly at 25 °C because of proton leakage, implying that it was distinguishable from the target (Fig. 6a).40 The proton leakage increased with respect to the strength of the BMHBs, but weakened with respect to the length of the PNIPAAm segment (Fig. S3†). The mismatches of AM and GM at 0.5 pg nL−1 could be distinguished from the target when using PN4D at 25 °C due to its high ratio of ssDNA:PNIPAAm segments. However, the resistivities of PN4D after hybridization with TM and CM at 0.5 pg nL−1 shifted to overlap the range of that with the target at 25 °C; therefore, TM and CM cannot be distinguished from that of the target due to their weaker BMHBs. These results indicate that the copolymer can distinguish the target from G and A mismatch, but not T and C mismatch at 25 °C. To identify the T and C mismatch, the temperature was increased to 80 °C to observe the changes in resistivities. The resistivity of blank PN20D ranged from 7.87 to 8.36 Ω cm, and decreased to the range from 7.34 to 7.79 Ω cm upon hybridization with the target at 80 °C. Because of proton leakage at 80 °C, the resistivities of PN20D after hybridization with AM and GM at 0.5 pg nL−1 decreased to the similar range as well, implying them to be undistinguishable from the target. In contrast, the resistivities of PN20D after hybridization with CM and TM at 0.5 pg nL−1 did not change significantly at 80 °C because the weak BMHBs were disrupted completely at 80 °C, implying them to be distinguishable from the target (Fig. 6b). These results suggest that selectivity for target detection was achieved by resistivity measurement at 25 and 80 °C to eliminate a false-positive mismatch. We increased the concentrations of AM, TM, GM, and CM for hybridization with the copolymer brushes until the resistivity could be distinguished from that of the target. Fig. 7 displays the lowest concentrations of distinguishable mismatch (LCDMs) from the target for all of the copolymer brushes at 25 and 80 °C. The LCDMs of AM, TM, GM, and CM from the target increased gradually upon increasing the length of PNIPAAm segment at 25 °C, verifying that the degree of proton leakage had a predominant effect on the LCDM. In contrast, the LCDMs of AM, TM, GM, and CM from the target decreased upon an increasing length of the PNIPAAm segments, indicating that thermal effects on the minor carriers determined the LCDM at 80 °C. These findings suggest that the mismatches of AM and GM could be distinguished efficiently from the target at temperatures below the LCST of PNIPAAm, whereas the mismatches of CM and TM could be distinguished predominantly at 80 °C, especially if the copolymer had a longer PNIPAAm segment. Notably, the thermal effect of the minor carriers was obvious at >80 °C. Furthermore, the variation in resistivity with respect to temperature was reversible for five cycles between 25 and 80 °C for all copolymer brushes, suggesting the stability of their resistivities to temperature. The electrical properties of the as-prepared copolymers may could be used to detect specific DNA sequences without the need to label them “smart materials”.
Fig. 5 Resistivities of PNIPAAm-b-ssDNA copolymer brushes (logarithm scale) plotted with respect to the hybridization concentration of the target (0.5–16 pg nL−1) at (a) 25 and (b) 80 °C. |
Fig. 6 Resistivities (logarithm scale) of (a) PN4D at 25 °C and (b) PN20D at 80 °C before and after hybridization with the target, AM, TM, GM, and CM at 0.5 pg nL−1. |
Fig. 7 LCDMs of AM, TM, GM, and CM from the target for hybridization with PNIPAAm-b-ssDNA copolymer brushes at (a) 25 and (b) 80 °C. |
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/c6ra28270a |
This journal is © The Royal Society of Chemistry 2017 |