Bei Jin‡
*,
Xiangzhong Li‡,
Xiaosong Zhou,
Xuan Xu,
Hailin Jian,
Mulan Li,
Keqi Guo,
Jinmin Guan and
Shanglong Yan
School of Chemistry and Chemical Engineering, Institute of Physical Chemistry, Development Center for New Materials Engineering & Technology in Universities of Guangdong, Lingnan Normal University, Zhanjiang 524048, PR China. E-mail: jinb@lingnan.edu.cn; Fax: +86-759-3183205; Tel: +86-759-3183205
First published on 17th March 2017
Jackfruit filum polysaccharide (JFPS) was extracted and confirmed to contain neutral and acidic polysaccharides, largely composed of acidic polysaccharides. Biodegradable JFPS–titanium dioxide (TiO2) nanocomposite films were fabricated using the solvent casting method combined with photocatalysis. The result of scanning electron microscopy (SEM) shows a uniform distribution of TiO2 nanoparticles into the gelatin matrix. Incorporation of TiO2 into the JFPS matrix significantly decreased the transparency, moisture content and total soluble matter. Surface hydrophobicity also decreased, the mechanical properties and thermal stability of the JFPS films improved. The JFPS/TiO2 nanocomposite films exhibited strong antibacterial activity against Escherichia coli and Staphylococcus aureus. The films incorporated with 3% (w/w) TiO2 showed the best mechanical properties and thermal stability, as well as excellent antimicrobial activity against Escherichia coli (78.9%) and Staphylococcus aureus (60.57%). The data of Fourier transform infrared spectra (FTIR) and X-ray diffraction (XRD) indicate that photocatalysis might contribute to the formation of the strong interfacial interaction between the JFPS matrix and TiO2 nanoparticles. Finally, these results demonstrated the feasibility of introducing photocatalysis to prepare nanocomposite films, and it is of significance in utilizing the JFPS and TiO2 to produce biodegradable nanocomposite films as packaging material in food and non-food industries.
Jackfruit (Artocarpus heterophyllus Lam.) originated in India and now is very popular throughout southeast Asia. Jackfruit is a medium-size evergreen tree that bears high yields of the largest known, succulent, aromatic, and flavorful fruit.4 Recently, jackfruit has attracted much attention due to its potential beneficial physiological activities, such as free radical scavenging, anti-microbial, anti-inflammatory, anticariogenic, antineoplastic, and hypoglycemic properties.5 Jackfruit seeds and other inedible portion discarded as waste are about 70% of whole plant and usually cause environmental pollution. As a byproduct, jackfruit filum contains redundant functional components such as polysaccharides, carotenoids and flavonoids which were believed to be closely associated with their biological activity.6 Extracting polysaccharide is a good way of using jackfruit filum. However, information about the films prepared from jackfruit filum polysaccharide is scarce.
Until now, for protein-rich and unsaturated fatty acid-rich foods, the poor mechanical and barrier properties as well as the limited antioxidative and antimicrobial activities of pure polysaccharide films do not satisfy the needs of the consumers.7 Therefore, the research works have been focused on the improvement of such properties by reinforcing biopolymers films with nanocomposite technology.8 Among them, titanium dioxide (TiO2) nanoparticles have drawn much attention in food packaging and biomedical applications because they are cheap, nontoxic and will provide protection against foodborne microorganisms as well as good heat stability.9 However, TiO2 particles are easy to aggregate and their incorporated materials usually lead to low stability and the reduction of film physical properties.10 Therefore, it is in high demand to develop highly effective green processing procedure to prepare novel active blend film incorporated with TiO2.
There is a growing scientific interest in the influence of photocatalysis on synthesis of compounds with improved properties. Photocatalysis provides a green chemical route for organic functional group transformation under mild conditions. In the past two decades, it has been successfully applied to organic synthesis such as hydroxylation of aromatic, oxidation of amine and carbonylation.11 Moreover, photocatalysis could be also used in the preparation of TiO2 nanocomposite material to improve antibacterial activity.12 However, to date, there is little information available on the fabrication of polysaccharides/TiO2 blend film obtained by photocatalysis.
In this work, we developed novel active packaging film made from a jackfruit filum polysaccharide incorporating TiO2 nanoparticles by photocatalysis. Moisture content, microstructure, and mechanical properties of the films were investigated. Antibacterial property of the films was evaluated. Finally, possible interactions between TiO2 nanoparticles and polysaccharides would be considered in the development of active packaging.
The conditions of PC were: the mobile phase was a mixture of ethyl acetate, pyridine, water, and acetic acid (5:5:3:1); the sugars were identified by spraying o-phthalic acid reagent (1.6 g of o-phthalic acid was dissolved in 100 ml of water saturated n-butanol, containing 0.9 ml aniline) onto the paper and heating at 100 °C for 2 min.14
The samples were hydrolyzed with 2 M trifluoroacetic acid (TFA) at 100 °C for 4 h. One part of the hydrolysate was acetylated and then measured by GC-MS (GC7820A, Agilent, USA) with an HP-5 quartz capillary column (30 m × 0.25 mm × 0.25 μm). The GC conditions were: helium carrier (gas flow rate at 1.0 ml min−1); selected for column temperature which increased from 50 °C to 250 °C at the rate of 10 °C min−1; temperature of the injection port was 260 °C; ion source: EI, 70 eV; the molecular weight range: 20–600.
The photographs of one pure JFPS film, JFPS/TiO2-0.5% and (c) JFPS/TiO2-4% nanocomposite films are shown in Fig. 1. Films formulated with and without TiO2 were clear and easy to peel from the casting plate. Films became less transparent and flexible with increased TiO2 concentration, but maintained a smooth surface without cracks or pores. Increasing the TiO2 concentration more than 4% (w/w) makes the JFPS films nonhomogeneous. Moreover, the pure JFPS film was transparent with a light pink colour. The JFPS/TiO2-0.5% was translucent with a light pink color. The JFPS/TiO2-4% was opaque with a white color. Transparency of the film is an important attribute, which influences the antioxidant capacity and acceptability of food in packaging systems. As shown in Fig. 2, with the addition of TiO2, the transparency of JFPS films significantly decreased, and that the transparency reached to a minimum level (22.9%) at concentration of 4% TiO2 nanoparticle (Fig. 2). This behavior can be probably due to non-uniform distribution of nanoparticles. Similar results were also reported by Zolfi et al. in kefiran–whey protein film incorporated with TiO2.19 The change in transparency may be caused by the presence of TiO2 in films. TiO2 could increase the whiteness of film at higher amounts, indicating that TiO2 might increase in crystallinity and decrease in amorphous regions in structure of films.
Fig. 1 Photographs of the (a) pure JFPS film, (b) JFPS/TiO2-0.5% and (c) JFPS/TiO2-4% nanocomposite films. |
Moisture content of the film is a very important attribute for food packaging application because packaging films have to maintain moisture levels within the packaged product. Table 1 shows MC values for films with different levels of TiO2 related to the control film. JFPS films incorporating TiO2 had slightly lower MCs than the control films, whereas no regular variation of MC was observed between the JFPS/TiO2 films with different levels of TiO2. Previous studies reported that incorporation of the TiO2 content of kefiran–whey protein isolate films also reduced moisture content in biocomposite films.20 Similarly, total soluble matter of JFPS films generally decreased with an increase in TiO2 nanoparticles content. These results were attributed to possible force between JFPS molecules and TiO2 nanoparticle, which reduced availability of hydroxyl groups in JFPS to interact with water.
TiO2/JFPS (w/w, %) | WC (%) | TSM (%) |
---|---|---|
a Results for each film are expressed as means ± standard deviation (n = 3). Values in the same column followed by the different letters indicate significantly differences (p > 0.05) according Duncan's multiple range test. | ||
0 | 22.6 ± 0.01a | 90.2 ± 0.07a |
0.5 | 18.8 ± 0.01c | 83 ± 0.02b |
1 | 21.2 ± 0.04b | 80 ± 0.05b |
2 | 21.6 ± 0.03ab | 68.5 ± 0.10c |
3 | 18.3 ± 0.05d | 67.3 ± 0.12c |
4 | 18.9 ± 0.04c | 59.8 ± 0.15d |
Contact angle (θ) of water with the film surface was used to evaluate the surface hydrophobicity of the film. The contact angle of JFPS films as a function of nanoparticle contents were shown in Fig. 3. The contact angle of pure alginate film was 53.7°, since the JFPS film is hydrophilic in nature. Moreover, the contact angle of JFPS film decreased with TiO2 incorporation and reduced to 42.9° in JFPS/TiO2-4% nanocomposites, which was mainly related to the increase in roughness of composite films, which was further confirmed by SEM. Other researchers reported similar results on the effects of nanoparticles on hydrophobicity of alginate and carboxyl methyl cellulose.21,22
Mechanical properties of a bionanocomposite material are highly dependent on the interfacial interaction between the nanofiller and biocomposite matrix.23 Tensile strength (TS) and elongation at break (EBA) of JFPS film and different contents of TiO2 nanocomposite film are shown in Fig. 4. Compared with JFPS film, TS of nanocomposite film increased significantly, EB decreased significantly with the increasing concentration of TiO2, which was in accordance with above MC analysis. These data indicated that the decreased moisture content would reduce the flexibility of the films. What's more, TiO2 nanoparticles could promote mechanical properties of JFPS film because TiO2 might strengthen the interfacial interaction through electrostatic attraction, hydrogen bonds and Ti–O–C bond between JFPS matrix and TiO2 nanoparticles induced by photocatalysis which was verified by XRD and FT-IR analysis and improve phase compatibility of JFPS matrix components which resulted in forming a stable three-dimensional polymeric matrix.24 Teymourpour et al. also noticed that tensile strength of soluble soybean polysaccharide film increased by 27.3% after the addition of 5% TiO2 nanoparticles.25
Fig. 4 Mechanical properties of JFPS/TiO2 nanocomposite films reinforced with different concentrations of TiO2. |
TGA was carried out to investigate the thermal performance of the nanocomposite films. TGA curves of the JFPS and JFPS/TiO2 films were presented in Fig. 5. The TGA curves of the films exhibited the weight loss pattern. TGA thermograms show similar behaviours for all studied films, with the presence of three thermal events. The first event (maximum peak occurred at around 65 °C) was attributed to water evaporation, which was about 3–8% of initial weight. The second event (maximum peak from 180 to 240 °C) resulted in a weight loss of approximately 40–45%, due to the degradation of glycerol and biopolymer polysaccharides. The degradation with about 45% of JFPS, nanocomposite films with different TiO2 concentration (0.5–4 w/w) presented temperature peaks at 227.1, 235.73, 242.51, 247.56, 257.64, and 271.1 °C, respectively. The introduction of nanoparticle (TiO2) significantly improved the thermal stability of JFPS films, which can be ascribed to the better thermal stability of TiO2 when compared with JFPS and to good interaction between TiO2 and JFPS. The third thermal event was observed around 300–350 °C, which was mainly related with the further oxidization and decomposition of the samples. After the final thermal decomposition, the residuals of pure JFPS, JFPS/TiO2 nanocomposite films with different TiO2 concentration (0.5–4 w/w) were 25.3, 28.1, 26.1, 33.1, 36.5 and 38.6%, respectively. This result indicated that photocatalysis might reinforce the interaction between JFPS molecule and TiO2 nanoparticle which contributed to improve the thermal stability of nanocomposite films. As TiO2 is crystalline; its crystallinity decreases the polar character of JFPS and the global water content in JFPS matrix which is agreement with above MC result. Similar results were also by Yang et al. who presented the decomposition onset temperatures of the nanocomposites shifted toward a higher temperature scope with increasing inorganic material content.26
Fig. 6 displays XRD data of the pure TiO2 and composite films with different TiO2 concentrations. The pure JFPS film is semi-crystalline in nature and shows a broad diffraction peak at 2θ = 22.57°. TiO2 had a significant peaks at 2θ = 25.3°, 37.9°, 47.8°, 54.5°, 63.1°, 69.4° and 75.2°, which contains both anatase phase and rutile phase. When the concentration of TiO2 nanoparticles in the film was less than 0.5%, XRD pattern was amorphous, but when the concentration increased and reached 2%, the obtained pattern was almost the same as that of the pure TiO2, which was in agreement with the transparency results. This result expressed that the crystal structure of TiO2 was not altered due to the presence of JFPS. Moreover, the intensity of the main characteristic peaks of TiO2 was higher as the concentration of TiO2 in the JFPS matrix increased. Comparison of peaks of the pure JFPS and nanocomposite films showed that the intensity of the peak at 2θ = 22.57° was gradually decreased and became border but no displace with the increasing TiO2 concentrations in the nanocomposite matrix. That might be the incorporation of nanoparticles would destroy the intra-molecules forces in the JFPS film such as hydrogen bonds, and then TiO2 nanoparticles can insert and disperse uniformly in the nanocomposite matrix, which strengthen the interaction between nanoparticles and JFPS molecules such as Ti–O–C bond induced by photocatalysis which was further confirmed by FT-IR analysis. Similar results have been observed with other TiO2-incorporated nanocomposites such as kefiran–whey protein/TiO2 and chitosan–whey protein/TiO2.20,21
The morphology of films is a very important characteristic as it could ultimately determine many properties of biodegradable materials. SEM patterns of the JFPS are shown in Fig. 7. The pure JFPS film had a homogeneous and smooth surface structure (Fig. 7A). The granular structure on the surface of composite films appeared when TiO2 particles were incorporated (Fig. 7B–D). The results showed that no significant changes were observed after incorporating TiO2 at the concentrations of 0.5–2% to bio-composite surface. This result indicated that photocatalyst might prompt the formation of the strong interfacial adherence between the JFPS and nano-TiO2 resulting in a good distribution of TiO2 in the polymeric structure, and was beneficial to the mechanical properties of the nanocomposite films. However, the discontinuous phase and some agglomerates can be observed in the microstructure as TiO2 concentration reached 4%. These results were agreed with XRD analysis. Similar results were reported for the surface micrographs of soluble soybean polysaccharide (SSPS)–TiO2 films containing different nano-TiO2 concentrations.25
Fig. 7 SEM micrographs of the surfaces of the pure JFPS film and JFPS/TiO2 nanocomposite films: (A) pure JFPS, (B) JFPS/TiO2-0.5%; (C) JFPS/TiO2-2%; (D) JFPS/TiO2-4%. |
The FT-IR spectra of neat JFPS and JFPS/TiO2 nanocomposite films exhibited distinctive peaks in the range of 4000–400 cm−1 (Fig. 8). Signals at 3420, 2920, 1620, 1400 and 1100 cm−1 were the typical characteristic of polysaccharides.27 A broad and intense peak at 3416 cm−1 and absorption band at 2936 cm−1 were observed in pure JFPS films which were related to –OH group and for –CH3 stretching vibrations. In addition, the peaks at 1617 and 1440 cm−1 were assigned to asymmetric and symmetric stretching vibrations of carboxyl groups present in the JFPS. The peaks of 1746 and 1261 cm−1 were attributed to the CO and C–O component of an ester bond, respectively. The region at 1200–850 cm−1 was assigned to stretching vibrations of C–O, C–C, ring structures and deformation of –CH2 group vibration. Moreover, the absorption peaks around 1100 cm−1 indicate that the sugar rings of the JFPS fractions were pyranose rings. There results indicated that the JFPS might consist of neutral and acidic polysaccharides, largely composed of acidic polysaccharides, which was in accordance with the report described by Zhu et al.6c As shown in Fig. 8, similar peaks were observed in pure JFPS and JFPS/TiO2 composite films. However, the intensity of the peak at 3416 cm−1 increased after composite formation with TiO2, suggesting that the nano-TiO2 interacted with JFPS by the hydrogen bond. Additionally, the intensity of band at 1440 cm−1 decreased and the peak position had red shift and that the intensity of the broad band at 535 cm−1 significantly decreased when TiO2 content exceeded 2%. The findings might be an indirect suggestion of the formation of Ti–O–C bonds between the JFPS and nano-TiO2 induced by photocatalysis, as shown in Fig. 9. In all, FTIR results confirmed the hydrogen bonding between the JFPS molecules and nanoparticles could increase when incorporated with TiO2 nanoparticles.
Fig. 8 FTIR spectra of the pure JFPS film and JFPS/TiO2 nanocomposite films: (a) pure JFPS, (b) JFPS/TiO2-0.5%; (c) JFPS/TiO2-1%; (d) JFPS/TiO2-2%; (e) JFPS/TiO2-3%; and (f) JFPS/TiO2-4%. |
The antimicrobial activity of JFPS composite films against bacteria E. coli and S. aureus was also tested and the results were presented in Fig. 10. JFPS film without added TiO2 showed fairly low antimicrobial activity, the inhibition rates of JFPS film for E. coli and S. aureus reached 6.87 ± 1.44% and 1.77 ± 0.46%, respectively. The antibacterial rates increased gradually for the JFPS film reinforced with increasing amounts of TiO2 nanoparticles. TiO2 is considered as antimicrobial agents with a broad spectrum of bacterial and fungal species. It has been believed that TiO2 could generate a strong oxidizing agent, hydroxyl radicals, which lead to lipid peroxidation and leakage of the cell membrane.25 This JFPS composite films had high antimicrobial activity due to the intermolecular force between TiO2 and JFPS which led to change in lattice of TiO2 nanoparticle and further generate more reactive oxygen species to inactivate microorganisms by causing cell lysis. In addition, the TiO2 incorporated JFPS composite films demonstrated stronger antimicrobial activity against E. coli than S. aureus which was opposite to that from the research reported by Teymourpour et al.25 This might be because cell wall structure of gram negative contains more lipoprotein and phospholipid and less peptidoglycan than that of gram positive bacteria which make the cell membrane more susceptible to attack by hydroxyl radicals leads to lipid peroxidation and protein denaturation. However, further research would be needed to illuminate the interaction between free radical and cell.
Fig. 10 The antibacterial effects on bacteria E. coli and S. aureus of nanocomposite films with various ratio of JFPS/TiO2. |
Footnotes |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/c6ra28648h |
‡ These authors contributed equally to this work. |
This journal is © The Royal Society of Chemistry 2017 |