Shaojie Chen,
Yefeng Yang*,
Ziyue Zhan,
Jinlei Xie and
Jie Xiong*
Department of Materials Engineering, Zhejiang Sci-Tech University, Hangzhou 310018, P. R. China. E-mail: yangyf@zstu.edu.cn; jxiong@zstu.edu.cn; Tel: +86-571-8684-3586
First published on 27th March 2017
In this work, we report the design and fabrication of hierarchical NiCo2S4@polypyrrole (PPy) core–shell hybrid nanosheet arrays on Ni foam as a novel battery-type electrode using a facile hydrothermal and electrodeposition strategy. The conductive and electroactive PPy layers are deliberately coated on the backbones of interconnected NiCo2S4 nanosheets to significantly boost the energy storage capacity. The resulting NiCo2S4@PPy hybrid electrode exhibits an enhanced areal capacity (800 μA h cm−2 at 5 mA cm−2) and good rate capability. An aqueous hybrid supercapacitor (HSC) device is assembled by employing NiCo2S4@PPy and activated carbon as the positive and negative electrodes, achieving high energy density (60.8 W h kg−1 at 200 W kg−1) and high power density (4362 W kg−1 at 31 W h kg−1), as well as excellent cycling stability (98.3% retention over 3000 cycles at 20 mA cm−2). Moreover, two HSC devices can easily light 38 LEDs efficiently, demonstrating the great potential of this core–shell hybrid nanostructure toward practical applications in energy storage devices.
Among various battery-type electrode materials, NiCo2S4 has intrigued particular research attention owing to the merits of low cost, facile fabrication as well as possessing richer redox reactions and higher electrical conductivity than the single component oxides and sulfides.24–29 In the past few years, many efforts have been devoted to further boosting the energy storage efficiency of NiCo2S4 by exploring various NiCo2S4-based core–shell nanostructures.30,31 For example, Xiao et al. reported the successful fabrication of NiCo2S4@CoxNi1−x(OH)2 nanotube/nanosheet arrays on carbon fiber papers with an improved areal capacity of 397 μA h cm−2 at a current density of 4 mA cm−2, which is about 3 times that of the pristine NiCo2S4.27 In another work, Fu and co-workers reported that the electrodeposition of ultrathin CoSx nanosheets on NiCo2S4 nanotube arrays on Ni foam can achieve a high areal capacity of 592.5 μA h cm−2 at 5 mA cm−2.32 Very recently, Niu et al. demonstrated the hydrothermal synthesis of NiCo2S4@Ni3V2O8 core/shell hybrid on Ni foam to obtain a high specific capacity of 142 mA h g−1 at 1 A g−1.33 Although notable progress has been made by the researchers, the designed construction of NiCo2S4-based core–shell nanostructures remains challenging, and many of the assembled HSC devices based on these materials still suffer from the less satisfactory electrochemical performance, especially in terms of achieving both high energy and power densities, which largely restricts their wide practical applications.
Herein, we report the design and fabrication of three-dimensional (3D) hierarchical NiCo2S4@polypyrrole (PPy) core–shell hybrid nanosheet arrays (NSAs) on Ni foam as binder- and additive-free electrodes for supercapacitors. The interconnected NiCo2S4 nanosheets were employed as excellent conductive backbones for docking electroactive materials, while the conducting polymer, PPy in this work, was chosen as the shell materials because of its high electrical conductivity (10–100 S cm−1) and fast redox reaction for charge storage.34,35 As expected, the coating of PPy nanosheets on the surface of NiCo2S4 can not only facilitate the electron transport in the system, but also provide larger surface area with more contribution of capacity from the shell materials. However, to the best of our knowledge, the combination of NiCo2S4 and PPy in an integrated electrode has been rarely reported.36 In this work, the optimized NiCo2S4@PPy core–shell hybrid NSAs can exhibit a high areal capacity of 800 μA h cm−2 at 5 mA cm−2, and a rate capability of 51.7% with current density increased from 5 to 100 mA cm−2. Remarkably, the aqueous HSC device based on this material displays a high areal capacity of 1528 μA h cm−2 at 5 mA cm−2, and excellent cycling stability of 98.3% over 3000 cycles at a high current density of 20 mA cm−2. Moreover, the HSC device can achieve a maximum energy density of 60.8 W h kg−1 at a power density of 200 W kg−1, and still retain 31 W h kg−1 at a high power density of 4362 W kg−1, suggesting the great potential of this hybrid electrode for high-performance energy storage devices.
The areal capacities for the battery-type electrodes were determined based on the following equation:
Qa = It/S |
The specific energy and power densities of the HSC devices were derived based on the total mass of active materials on both electrodes according to the following equations:37
P = E/t |
Fig. 1 Schematic illustration of the synthetic procedure for NiCo2S4@PPy core–shell hybrid NSAs on Ni foam. |
The crystalline structure and phase purity of the hybrid composite were probed by XRD measurement. Fig. 2 shows the typical XRD pattern of the NiCo2S4@PPy hybrid NSAs on Ni foam substrate. The diffraction peaks at 2θ values of 31.6°, 38.3°, 47.4°, 50.5° and 55.4° can be readily identified as the (311), (400), (422), (511) and (440) planes of the NiCo2S4 phase (JCPDS no. 43-1477), while the three dominant peaks at 44.7°, 52.1° and 76.5° are attributed to the Ni foam substrate (JCPDS no. 87-0712).38 Apart from these peaks, a broad peak centered at ca. 23° arising from the coated PPy phase is also detected, which is distinctly in agreement with the reported literatures on PPy-based composites,39–41 reflecting the poor crystallinity of the PPy layers within the hybrid composite.
The surface morphologies of the products were characterized by FESEM. For the pristine NiCo2S4 (Fig. 3A and B), it is revealed that the whole Ni foam skeleton has been covered by high-density of NiCo2S4 nanosheets with an average wall thickness of ca. 50 nm and lateral size ranging from 1 to 2 μm. These NiCo2S4 nanosheets directly grown on Ni foam are observed to interconnect with each other to form a 3D porous network with adequate interspaces among them, which can be utilized as ideal conductive backbones to support additional electroactive materials. After the electrodeposition, as shown in Fig. 3C and D, one can see that the NiCo2S4 backbones have been entirely wrapped by a thin film of PPy shell materials with total thickness increased to ca. 120 nm, forming the desirable hierarchical NiCo2S4@PPy core–shell hybrid nanostructures. Despite the integration of PPy into the composite, the array structures are well retained. Moreover, high-magnification SEM image (Fig. S2†) indicates that the PPy shell materials are in fact composed of many tiny nanosheets, which can be further confirmed by TEM.
Fig. 3 Typical SEM images of (A and B) pristine NiCo2S4 and (C and D) NiCo2S4@PPy hybrid NSAs at low-and high-magnification, respectively. |
Further insights into the morphology and microstructure of the products were revealed by TEM and HRTEM. Fig. 4A shows a typical TEM image of an individual NiCo2S4 nanosheet with relatively smooth surface. More details are clearly illustrated by HRTEM. As shown in Fig. S3,† the NiCo2S4 nanosheets are observed to possess many crystalline particles and mesopores in them, demonstrating their polycrystalline characteristics. The HRTEM image in Fig. 4B exhibits two sets of visible lattice fringes with an interplanar spacing of 0.34 and 0.28 nm, corresponding well to the (220) and (311) planes of cubic NiCo2S4 phase, respectively, as supported by previously reported literatures on NiCo2S4.26,42 The TEM image taken from the NiCo2S4@PPy hybrid NSAs (Fig. 4C) confirms that the surface of NiCo2S4 nanosheet has been successfully deposited with a layer of ultrathin and interconnected PPy nanosheets, which can provide more electroactive sites and greatly facilitate the charge transfer in the system to boost the energy storage efficiency. HRTEM studies (Fig. 4D) reveal the distinct interface between the NiCo2S4 core and amorphous PPy shells with a layer thickness of ca. 30 nm, unambiguously testifying the core–shell heterostructures. In addition, the EDS mapping analysis by HAADF-STEM (Fig. 5) shows that the constituent elements of C, N, Ni, Co and S can be detected throughout the observed nanosheet region, suggesting the homogenous distribution of PPy shell materials on the whole NiCo2S4 backbones, which is consistent with TEM measurement. Moreover, FTIR has been utilized to explore the functional organic groups from PPy layers, and the result is illustrated in Fig. S4,† which clearly demonstrates the successful coating of PPy layers on the NiCo2S4 nanosheets.
Fig. 5 (A) Typical HAADF-STEM image of an individual NiCo2S4@PPy hybrid nanosheet, and (B–F) corresponding EDS mapping analysis. |
The superior electrochemical properties of hierarchical NiCo2S4@PPy core–shell hybrid NSAs for supercapacitors were first investigated in a three-electrode system with 2 M KOH solution as the electrolyte. The CV curves of the pristine NiCo2S4, PPy and NiCo2S4@PPy hybrid electrodes as well as bare Ni foam were tested at a scan rate of 10 mV s−1 with a potential window ranging from −0.1 to 0.6 V, as shown in Fig. 6A and S5.† It should be pointed out that the contribution of Ni foam substrate to the overall capacity can be neglected since there is almost no evident redox peaks from Ni foam. For the pristine NiCo2S4, a pair of broad peaks arising from the redox reactions of NiCo2S4 in alkaline solution is visible, suggesting the faradaic characteristics of battery-type electrodes,8,43 which is quite different from the EDLC-type and pseudocapacitive such as MnO2 (ref. 44) and RuO2 (ref. 45) electrodes with nearly rectangular CV shapes. The mechanism of the electrochemical reaction can be attributed to the faradaic redox process of Co2+/Co3+/Co4+ and Ni2+/Ni3+ based on the following equations:36,42 NiCo2S4 + OH− + H2O ↔ NiSOH + 2CoSOH + 2e−, CoSOH + OH− ↔ CoSO + H2O + e−. After the coating of PPy nanosheets, the PPy shells are able to contribute additional capacity via doping/de-doping in alkaline solution.46 As expected, the NiCo2S4@PPy hybrid electrode exhibits much increased CV integrated area than the pristine NiCo2S4 and PPy electrodes, indicating the largely enhanced energy storage capacity for the hybrid electrode.47 Fig. 6B compares the galvanostatic discharge curves of these electrodes at the same current density of 10 mA cm−2. As observed, the NiCo2S4@PPy hybrid electrode displays a much longer discharging time than the other electrodes, further demonstrating the improved electrochemical performance of the hybrid electrode through PPy coating. Fig. 6C displays the CV curves of the NiCo2S4@PPy hybrid electrode recorded at various scan rates ranging from 2 to 20 mV s−1. The shapes of these CV curves show no significant changes as the scan rate increases, suggesting that this hybrid electrode is favorable for high-rate energy storage process.48 Fig. 6D presents the galvanostatic discharge curves of the NiCo2S4@PPy hybrid electrode at different current densities varying from 5 to 100 mA cm−2. The areal capacities of the NiCo2S4@PPy hybrid electrode are calculated from the discharge curves and plotted as a function of current density in Fig. 6E with pristine NiCo2S4 and PPy also included for comparison. Within the whole current density range, the NiCo2S4@PPy hybrid electrode delivers a much higher areal capacity than that of pristine NiCo2S4 and PPy (the areal capacity of PPy rapidly decreases to zero at a current density of 30 mA cm−2). Remarkably, the NiCo2S4@PPy hybrid electrode displays a high areal capacity of 800 μA h cm−2 at a current density of 5 mA cm−2, which is about 2.1 times that of pristine NiCo2S4 (383.9 μA h cm−2) and nearly 74 times that of PPy (10.8 μA h cm−2) under the same condition. This result is also much higher than those reported values on core–shell electrodes on Ni foam, such as NiCo2O4@NiCo2O4,15 NiCo2S4@MnO2,31 ZnCo2O4@PPy,39 NiCo2O4@PPy,41 NiCo2O4@PEDOT,46 NiCo2S4@Ni(OH)2,49 NiMoO4@Co(OH)2,50 NiCo2O4@CoxNi1−x(OH)2.51 Moreover, even at a current density as high as 100 mA cm−2, the NiCo2S4@PPy hybrid electrode still manifests a high areal capacity of 413 μA h cm−2 with 51.7% retention of the initial capacity, which is about 1.6 times that of pristine NiCo2S4 (265 μA h cm−2). The enhanced electrochemical properties for the hybrid electrode can be explained by the integration of NiCo2S4 and PPy in such a unique hierarchical structure as well as the distinct synergetic contribution from the core–shell components.
To further understand the superior electrochemical performance of the NiCo2S4@PPy hybrid electrode, EIS measurements were carried out in a frequency range of 0.01 Hz to 100 kHz. Fig. 6F presents the Nyquist plots of pristine NiCo2S4, PPy and NiCo2S4@PPy hybrid electrodes. In the high frequency region, the real axis intercept of the curve indicates the bulk resistance, and the semicircle diameter reflects the charge transfer resistance, while in the low frequency region, the straight slope of the curve shows the Warburg resistance (ion diffusion resistance).52,53 As shown in Fig. 6F, the NiCo2S4@PPy hybrid electrode exhibits a decreased bulk resistance than that of pristine NiCo2S4 and PPy and a minimized charge transfer resistance, suggesting the improved electrical conductivity of NiCo2S4 through the coating of PPy layers. Besides, the very similar slope of straight line for these electrodes implies that the interconnected core–shell nanostructures are highly accessible for ion diffusion into the electrodes. Owing to the fast electron transport and facile ion diffusion kinetics, the designed formation of NiCo2S4@PPy hybrid NSAs shall hold great promise as electrodes for high-performance HSCs.
To evaluate the electrochemical performance of the NiCo2S4@PPy hybrid NSAs in real devices, an aqueous HSC device was fabricated by employing the NiCo2S4@PPy and AC as the positive and negative electrodes, respectively, as schematically illustrated in Fig. 7A. The CV curves of the NiCo2S4@PPy and AC electrodes were first investigated in a three-electrode system (Fig. 7B) with a voltage window of −0.1 to 0.6 V and −1.0 to 0 V, respectively. It can be thus inferred that the as-fabricated NiCo2S4@PPy//AC HSC device is capable of affording a stable operating voltage of 1.7 V. Fig. 8C shows the CV curves of the NiCo2S4@PPy//AC device recorded at various scan rates from 5 to 100 mV s−1, which reveals the combined contribution of a battery-type faradaic electrode and a capacitor-type electrode to the CV behaviors. Fig. 7D displays the galvanostatic discharge curves of the device under different current densities ranging from 5 to 100 mA cm−2. The NiCo2S4@PPy//AC HSC device delivers an areal capacity of 1528 μA h cm−2 at 5 mA cm−2, and still retains 710 μA h cm−2 at a high current density of 100 mA cm−2, as illustrated in Fig. 7E. The cycling stability of the HSC device is very important and also evaluated by repeated charge–discharge tests at 20 mA cm−2. As shown in Fig. 7F, the overall areal capacity of the device increases at the beginning of several hundred cycles due to the slow activation of the electrode materials, and then gradually decays with increasing cycles. After 3000 cycles, the HSC device still exhibits 98.3% retention of the initial value and nearly 100% coulombic efficiency, demonstrating the outstanding long-term cycling stability and good electrochemical reversibility. This fact can be also reflected by the SEM image of NiCo2S4@PPy electrode of the HSC device after 3000 cycles, with slightly changed morphology and structure as shown in Fig. S6.†
The energy density and power density are two vital parameters generally used to evaluate the energy storage devices for practical applications. Fig. 8A displays the Ragone plots of as-fabricated NiCo2S4@PPy//AC and NiCo2S4//AC devices, and data of some previously reported devices in aqueous electrolyte are also provided for comparison. It is worth noting that the NiCo2S4@PPy//AC device achieves a maximum energy density of 60.8 W h kg−1 at a power density of 200 W kg−1, and is still capable of retaining 31 W h kg−1 even at a high power density of 4362 W kg−1, which is about 2 times that of NiCo2S4//AC (30.3 W h kg−1 at 274 W kg−1, and 17.7 W h kg−1 at 5554 W kg−1). Notably, the obtained energy density of the NiCo2S4@PPy//AC device is comparable or even superior to many of the recently reported aqueous HSC devices, such as CoO@PPy//AC (43.5 W h kg−1 at 87.5 W kg−1),35 NiCo2S4@PPy//AC (34.6 W h kg−1 at 120.2 W kg−1),36 NiCo2S4@Ni(OH)2//AC (53.3 W h kg−1 at 290 W kg−1),49 NiCo2O4@CoxNi1−x(OH)2//CMK-3 (31.2 W h kg−1 at 396 W kg−1),51 NiCo2O4@NiMoO4//AC (21.7 W h kg−1 at 157 W kg−1),52 NiCo2S4@Co(OH)2//AC (35.9 W h kg−1 at 400 W kg−1),54 Co3O4@PPy@MnO2//AC (34.3 W h kg−1 at 80 W kg−1)55 and TiO2@Ni(OH)2//mesoporous carbon (53.5 W h kg−1 at 77.1 W kg−1).56 To further highlight the high energy and high power performance, two NiCo2S4@PPy//AC devices are assembled in CR-2025 coin cells and connected in series. As shown in Fig. 8B, the devices can easily power 38 red LEDs with the characters of “2016” brightly after a short time of charging, strongly suggesting the great potential in practical applications as advanced energy storage devices.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/c6ra28693c |
This journal is © The Royal Society of Chemistry 2017 |