B. R. Pistillo*,
K. Menguelti,
D. Arl,
F. Addiego and
D. Lenoble
Department of Materials Research and Technology, Luxembourg Institute of Science and Technology, 5, Avenue des Hauts Fourneaux, L-4326 Esch sur Alzette, Luxembourg. E-mail: tillo@list.lu; Fax: +352 27 58 85; Tel: +352 275.888.586
First published on 30th March 2017
Efficient deposition of polymers on 3D substrates is a key point for many applications where a high surface area is required. Smart textiles based on conductive fibers is one of the most attractive domains where conformal polymer deposition is essential. In this frame, plasma radical assisted polymerization via chemical vapour deposition (PRAP-CVD), a solvent-free technique, has been demonstrated to be able to deposit highly uniform poly(3,4-ethylenedioxythiophene) (PEDOT) films. Low temperature of the substrate (<100 °C) and medium vacuum (<50 Pa) combined with good functionality of the films allow the application of PRAP-CVD to a wide range of complex substrates. Polyethylene terephthalate wipers were covered with PEDOT by PRAP-CVD to develop textile-based devices. PRAP-CVD versatility goes beyond the current vapour/solution-based techniques as shown in this work.
Plasma radicals assisted polymerization via CVD (PRAP-CVD) is emerging as an efficient alternative to conventional vapour-based technique to synthesise and deposit conjugated polymers.20 The low deposition temperatures, below 100 °C, allow polymers to be directly synthesised on a wide range of substrates, including paper and plastic, without any thermal degradation. Additionally, the PRAP-CVD does not require post-deposition rinsing procedure. In this study we demonstrated the advantage of depositing PRAP-CVD PEDOT directly on the fabric. Polyethylene terephthalate (PET), more commonly referred to as polyester, was chosen as reference textile since it is one of the most commonly used polymers in textile industry both as fibres and fabrics because of its high strength, low moisture absorption, and resistance to shrinkage which fulfil fibre industry specifications.
We combined the advantage of PRAP-CVD, as substrate-independence process and the conformality of produced film, to obtain efficient conductive PET fabric. PEDOT did not alter functional properties of the textile and withstand substrate drawing. This study highlights the potential of PRAP-CVD as a scalable and commercially feasible method with unique capabilities in terms of conformality.
The polymerization mechanism of EDOT to form PEDOT is described elsewhere.21 In essence, the production of bromine plasma radicals began a free-radical polymerization of the EDOT at the substrate surface. The polymerization stopped when last α′ position available was brominated. The obtained polymerization was firstly attested by optical microscopy (OM), as reported in Fig. 2. Before the deposition the PET wipe appeared white while just after the process, it changed colour appearing bluish. In the oxidized state, cations generated every five EDOT monomer segments are charge balanced with anions in the vicinity. The electronic arrangement is shown schematically in Fig. 3. The counter ion for PRAP-CVD is bromine. The unpaired electrons are delocalized along the PEDOT backbone, resulting in conductive behaviour of PEDOT. In this highly energetic state, the electrons absorb mostly low-energy near-infrared light and are relatively transparent to visible light. In the reduced state, the electrons are most stable in the conjugated alternating single/double bond configuration. Due to resonance, the electrons are delocalized over a few polymer segments. The conjugated electrons are at a lower energy than unpaired electrons, and absorption is shifted into the higher energy visible region, resulting in the dark colour.22,23 The conformity of film on the fibres is a key point in the list of industrial requirements. Conductive PEDOT films were deposited on standard PET fabric to demonstrate functional conformal films. Scanning electron microscopy (SEM) investigation was carried out to prove the effectiveness of the technique. A comparison before and after PRAP-CVD process is reported in Fig. 4. Correspondence of the textile morphology between the uncoated and coated sample illustrated the high conformal coverage of the fibres with thin film of polymer (Fig. 4a and b). The presence of PEDOT sustained by the changing in colour and preserved morphology was confirmed by Energy Dispersive X-ray spectroscopy (EDX) in Fig. 4c and d, respectively. In the spectrum of PET, peaks of carbon (C) Kα at 0.3 keV and oxygen (O) at 0.5 keV were detected while the spectrum of fibres treated via PRAP-CVD highlighted the presence of sulphur (S) at 2.3 keV and bromine (Br) at 11.9 keV. Sulphur as well as carbon and oxygen were attributed to the chemical composition of EDOT while bromine was present as dopant. PEDOT film resulted in defect/pin-hole free, as attested by the high magnification SEM micrographs. In order to deeply prove this peculiarity of PRAP-CVD, a stripe of PET fabric covered with PEDOT was cut by means a scalpel and analysed by SEM. In Fig. 5, micrographs of the same PEDOT/PET area, recorded at different magnifications, are reported (Fig. 5a and c). The cut induced a physical convergence of fibres. The light area could be attributed to the PEDOT which responded differently from PET to the irradiation of the electron beam. The presence of PEDOT was also confirmed by the rip of fibres owing to movement of scalpel. A video attesting this behaviour is present in ESI† document. The same images were also artificially coloured by Image J software (Fig. 5b and d) to easily identify the layer of PEDOT which conformably surrounded each fibre although the convergence of fibres.
Fig. 2 Optical microscopy images of (a) untreated knitted PET fabric microstructure appearing with a white colour, and (b) knitted PEDOT/PET fabric microstructure appearing with a blue one. |
Fig. 3 Electronic arrangement of PEDOT doped with bromine. Oxidised PEDOT showed a light sky blue colour. |
Following FIB cross-sectioning step, an accurate thickness measurement of film deposited all around the textile fibres was determined. A thickness of (215 ± 10) nm allowed to establish a deposition rate of 6 nm min−1. This level of coating quality is unparalleled to current wet and dry PEDOT synthesis.24,25
Raman investigation was carried out to prove PEDOT polymerization by determining the vibrational modes of spectra. The Raman spectra of PEDOT/PET and of the untreated PET, measured at excitation wavelengths of 633 nm, are displayed in Fig. 6. In the Raman spectrum of pure PET fabric (Fig. 6a), two strong characteristic bands appeared at 1729 cm−1 and 1615 cm−1, which corresponded to the C–O stretching vibration and benzene ring stretching vibration, respectively. Weak band at 1415 cm−1 could be attributed to the aromatic ring C–C stretching vibration and –OCH2– wagging vibration. The bands that identified methylene group, owing to the C–H deformation vibration and the CH2 wagging vibration, were observed at 1461 cm−1 and 1290 cm−1, respectively. The asymmetric C–O–C stretching also contributed to the last band. The band at 1182 cm−1 was owing to the symmetric C–O–C stretching. The ester C(O)O bending mode was attributed to the band at 859 cm−1 while the band generated by the in-plane deformation vibration of the C(O)O group, characteristic for aromatic esters, was detected at 632 cm−1.25–27 The spectrum of PEDOT/PET in Fig. 6b showed low-intensity bands at 579 cm−1 and 989 cm−1, ascribed to the oxyethylene deformation. The band at 707 cm−1 and 1262 cm−1 corresponded to symmetric C–S–C deformation and Cα–Cα′ (inter-ring) stretching modes, while that at 1370 cm−1 was attributed to the Cβ–Cβ stretching. The symmetric CαCβ (–O) stretching was assigned at 1426 cm−1 and the asymmetric CαCβ stretching at 1514 cm−1.21,28 The other bands could be attributed to the presence of substrate beneath.
It was also possible to determine chemical states of PET and PEDOT/PET C 1s respectively, by X-ray Photoelectron Spectroscopy (XPS), as presented in Fig. 7. The atom in the untreated PET spectrum, Fig. 7a, was present in three chemical states, reflecting the presence of the three peaks: C1 at binding energy of 284.5 eV that corresponded to C–C/H bond (aliphatic/aromatic carbon atoms), C2 at 286.0 eV attributed to C–O bond (methylene carbon atoms singly bonded to oxygen), and C3 at 288.5 eV recognised as signal owing to –COO– bond (ester carbon atoms). Last, the broad small peak at 291 eV corresponded to the π–π* shake-up transition associated with the aromatic ring of the PET.29 The best fitting procedure allowed attributing the following percentage areas: 54.2% C1, 24.6% C2, 14.6% C3, and 6.6% shake-up. In Fig. 7b, the distribution of functional groups of PEDOT C 1s showed three different components: C1 represented C–C/H bonds, depicted at 284.4 eV, C2 attributed to C–S at 285.5 eV and C–O at 286.1 eV. An asymmetrical peak at about 288 eV owing to the contribution from the π → π* shake-up transition and positively polarized or charged carbon was also identified. Peak areas were calculated as 34.8% for C–C/H, 42.5% for C–S, 17.3% for C–O and 5.4% for the shake-up.30 Best-fitting procedure was also applied to core-level of O 1s and S 2p. In particular, S 2p core-level spectrum corresponded to single sulphur bonding environment in PEDOT with a spin-split doublet, 2p1/2 and 2p3/2 separated by 1.18 eV in binding energy and an area ratio 1:2, as presented elsewhere.21 The presence of the asymmetric tail at higher binding energy was related to the doping process, in which the delocalized π-electrons in thiophene ring broaden the binding energy spectrum of the sulphur atom.31 The quantitative analysis of PEDOT film showed the followed atomic percentage of 66% C, 21% O, 9% S, and 4% Br.
Fig. 7 XPS C 1s high resolution spectra of (a) PET and (b) PEDOT/PET and relatively chemical states. |
The resistance of PEDOT coating to drawing was investigated by in situ tensile testing of PET fabric in an environmental pressure SEM at a temperature of 20 °C and at a strain rate of 0.0025 s−1. The typical stress–strain curve of PEDOT/PET subjected to tensile testing is shown in Fig. 8. A comparison between the raw and covered fabrics was reported. In the case of PEDOT, three steps were identified: (i) from 0% to about 9% of strain, a marked increase of stress was observed certainly due to the intrinsic stiffness of the fabric, (ii) from 9% to 80% of strain, a stabilisation of stress was noted probably owing to the progressive rearrangement of the fabric fibres around the knits, and finally (iii) above 80% of strain, a high increasing of the stress was observed reflecting one more time a high tensile strength. This last stage of strain-hardening could suggest the drawing of the fibres oriented in the tensile direction and the drawing of the knits exhibiting resistance to the imposed strain. Note that the tensile behaviour of the different fabrics was only representative up to 90% of strain, and then the tensile behaviour was not repeatable due to activation of different mechanisms of edge fabric damage and fabric rupture yielding to different intensities of strain-hardening. A quite similar tensile behaviour could be identified in the case of raw fibres, attesting the low influence of PEDOT on the fabric mechanical properties.
Fig. 8 Typical stress vs. strain curves of untreated PET fabric and PEDOT/PET fabric at 0.0025 s−1 and 20 °C. |
SEM investigation was performed to check possible damage of fibres during and after the traction. As reported in Fig. 9a, SEM micrographs of fabric at its maximum strain of 175% was recorded and compared with that of the fabric after unloading corresponding to a strain of 100%, Fig. 9b. The film did not show any evidence of damage or morphology change indicating that the film withstand drawing with a high elasticity. Even in the extreme case of locally broken PET fibres, PEDOT adhered strongly to the PET, since no crack was detected on the part which remained on the substrate.
Fig. 9 SEM images of PEDOT/PET at (a) strain of 175% before unloading and (b) relaxed state after unloading corresponding to a strain of 100%. |
This finding demonstrated that PRAP-CVD allowed a high conformal deposition bypassing the poor connectivity and the delamination phenomena common to the other techniques.24 For all experiments run any modification in the morphology of samples was detected during the unloading stage. This result could support the hypothesis that PEDOT can also withstand the relaxation of PET fabric, probably due to a high intrinsic elasticity.
Fabric properties, in terms of conductivity, were modified with the presence of PEDOT, as anticipated by SEM analyses. Any resistance could be measured on the raw PET substrate, while when it was processed an electrical resistance of 35.19 MΩ was found. Similar values in terms of sheet resistance were measured also after drawing, attesting the high degree of elasticity of film chains. Considering the thickness of film measured via cross-section SEM, the conductivity of film was estimated to be 3 S cm−1, which is a promising value considering the uncountable advantages of PRAP-CVD compared to the other CVD techniques.
Finally, the size of sample is also a parameter which diversify PRAP-CVD to the current CVDs, samples up (15 cm × 15 cm) can be treated. In the Fig. 10, an example of PEDOT/PET (13 cm × 13 cm) has been reported.
A large area of sample could covered with PEDOT revealing a quite good degree of uniformity. The homogeneous temperature all over the substrate is a key aspect of PRAP-CVD and it is obtained by a good balance between the vacuum and the adhesion of the sample to the sample holder.
In order to facilitate the readability of paper an ESI† wad added.
3,4-Ethylenedioxythiophene (EDOT, 97%) and bromine (puriss. p.a., ≥99.0%), Sigma-Aldrich (Belgium), were used as received to deposit PEDOT film. The deposition took place in the PRODOS-200 PVPD™ R&D System-β version (AIXTRON SE, Herzogenrath, Germany).
EDOT monomer vapour was delivered into the reactor by a TriJet® (φEDOT = 4.2 × 10−3 mol min−1) and bromine by a bubbler system (φBr2 = 6.8 × 10−4 mol min−1). The different pathways allowed a well separated injection of monomer and oxidant. Any mix occurred whilst mingling the respective jet in the reactor close to the surface of the substrate. The substrate temperature was set to 80 °C while the reactor pressure was kept constant at 390 mTorr by a throttle valve.
Surface physical–chemical characterizations as XPS, EDX and Raman spectroscopy highlighted the homogeneous covering of PEDOT all around the fabrics and its independence from the kind of substrate. The behaviour of PEDOT when undergone to mechanical stress, revealed that the film withstand drawing with a high elasticity. By this technique is therefore possible modify only the surface of substrate without interfering with its bulk properties.
The conformal nature of PRAP-CVD PEDOT, highlighted by SEM micrographs, make an easy possibility the modification of objects having complex shapes.
In conclusion, PRAP-CVD polymerization produced conformal coatings, which precisely followed the geometry of the underlying substrate independently from its nature. The mild experimental conditions permitted its application to a wide range of substrates. The deposition, developed in a pre-industrial machine, can be carried out on 8-inch silicon wafer as well as 15 cm × 15 cm squared samples.
To our best knowledge, this is the most conformal way to deposit polymeric film all around textiles. This work also highlighted the industrial maturity of this novel technique and the easy scaling up of this process featuring highly competitive growth rate compared to other vapour phase growth of PEDOT thin-films.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/c7ra00343a |
This journal is © The Royal Society of Chemistry 2017 |