Zhiyong Liu*ab,
Tingwei Heab,
Kaikai Liua,
Qinqin Zhia and
Mingjian Yuan*abc
aDepartment of Physics and Materials Science, Henan Normal University, Xinxiang 453007, China. E-mail: zyliu01@163.com
bHenan Key Laboratory of Photovoltaic Materials, Xinxiang 453007, China
cDepartment of Chemistry, Nankai University, Tianjin 300071, China. E-mail: yuanmj@nankai.edu.cn
First published on 17th May 2017
In this paper, we have reported a high-performance inverted planar perovskite solar cell (PSC) with double-decked hole transport layer (HTL) sandwiched between the indium tin oxide (ITO) electrode and the perovskite photoactive layer. The double-decked HTL film is fabricated by coating inorganic vanadium oxide (V2Ox) layer and poly(3,4-ethylene dioxy-thiophene)–poly(styrene sulfonate) (PEDOT:PSS) layer. In this study, double-decked V2Ox/PEDOT:PSS HTL film can improve the optoelectronic properties of PSC device. It has been found that the double-decked V2Ox/PEDOT:PSS film plays a crucial role in enhancing charge transfer rate and suppressing electron–hole pair recombination. The valence of vanadium in the V2Ox has been changed by adjusting the molar ratio of V2O5 to H2O2. The PSC can reach its best performance when V2O5 and H2O2 react at a molar ratio of 1:60. In addition, the concentration of the V2Ox aqueous solution has also been changed to optimize performance of PSC. Hence, the device with double-decked V2Ox/PEDOT:PSS HTL film can increase the power conversion efficiency (PCE) to 15.86%, higher than that of reference device with PEDOT:PSS (13.56%). Besides, compared with reference device, our device has a better repeatability in the preparation process.
The poly(3,4-ethylene dioxy-thiophene)–poly(styrene sulfonate) (PEDOT:PSS) is usually used as HTL to enhance crystallinity of the perovskite layer film.20–22 We find it easy to collect the holes via the PEDOT:PSS layer, because PEDOT:PSS has many advantages over others such as good conductivity, smooth morphology, high work function (WF) and high transparency.23 The PCE of the inverted planar PSCs has been improved significantly by PEDOT:PSS HTL film. What merits much attention is that lots of research works have been carried out to enhance performances of PSCs, except PEDOT:PSS HTL film.24,25 Some researches have been conducted to use inorganic transition metal oxides including nickel oxide (NiOx),26–29 lead sulfide (PbS),30 and molybdenum oxide (MoOx)31–33 as the HTL film. The conduction levels of the oxides are much higher than the lowest occupied molecular orbital (LOMO) of the organic layers, which can prevent electrons from transporting in the wrong directions and improve the photo current of PSCs. However, most transition metal oxides films are thermally evaporated onto the substrates in vacuum and will hardly be applied to commercial production process of PSC devices due to its high cost.34,35 Recently, some techniques based on a lower-cost, simpler and more controllable approach have been reported.36 Some solution-processed bilayer HTLs have been used in solar cells, such as graphene oxide (GO)/PEDOT:PSS,37 MoO3/PEDOT:PSS,38 and PEDOT:PSS/vanadium oxide (V2Ox).39 Whereas, these cells do not show a higher PCE. Here we use double-decked V2Ox/PEDOT:PSS as HTL of PSCs, by contrast, the higher efficiency and better repeatability of the devices has been achieved by changing the valence of vanadium of double-decked V2Ox/PEDOT:PSS film.
The vanadium pentoxide (V2O5) and its derivative compounds have been researched intensively due to their redox activity.40–42 The V2Ox can be obtained by a simple method of synthesis that uses V2O5 and hydrogen peroxide (H2O2) as starting material at a low temperature. Through this method, the vanadium element produces a variety of binary compounds with the chemical general formula VO2+x (−0.5 ≤ x ≤ 0.5), such as V2O3, VO2, V2O5, V3O7, V4O9, V6O13.43 The V2Ox with different valences can be prepared by controlling the molar ratio of V2O5 to H2O2. In this work, the double-decked V2Ox/PEDOT:PSS films prepared by spin-coating V2Ox and PEDOT:PSS solution can serve as the HTL to enhance charge transfer rate and suppress electron–hole pair recombination in PSCs. Here we report a high-performance inverted planar PSC device with the structure of ITO/V2Ox/PEDOT:PSS/CH3NH3PbI3−xClx/the phenyl-C61-butyric acid methyl ester (PCBM)/Ag. The maximum PCE of 15.86% has been achieved by controlling the optimum concentration of the V2Ox solution. An average power conversion efficiency (PCEAVE) of has been increased significantly from 11.85% (the PCEAVE of 30 reference devices with PEDOT:PSS HTL) to 14.97% (the PCEAVE of 120 controllable devices with the double-decked V2Ox/PEDOT:PSS HTL).
V2O5 + H2O → V2O5·nH2O | (1) |
The reaction has increased acidity of the solution.49 The V2O5·nH2O molecule is dissociated by adding H2O2, forming the peroxovanadate. Therefore, the degree of acid hydrolysis is controlled by acidic precursor phase solution (eqn (2)).50
V2O5·nH2O + H2O2 → H3VO4 | (2) |
The peroxovanadate is not very stable in aqueous solution. The partial stability of peroxovanadate in metastable phase is achieved when aqueous solution is let set for 10 h or more (partially oxidation of V5+ to V4+ ions), resulting in the formation a mixture of vanadium oxide (eqn (3)).
H3VO4 → V2Ox·nH2O | (3) |
XPS was used to investigate composition of the V2Ox thin film with the optimal molar ratio of V2O5 to H2O2. High resolution XPS spectrum corresponding to V is shown in Fig. 1a. As shown in the images, the V 2p spectrum can be well fitted with 2p1/2 and 2p3/2 doublets by a Gaussian function, which corresponds to vanadium in two different oxidation states (V5+ and V4+). Two peaks at the binding energy (BE) of 517.7 and 525.1 eV are corresponding to the 2p doublet of V5+. And the other two peaks at the BE of 516.7 and 524.1 eV are correspond to the 2p doublet of V4+ respectively. The atomic concentration ratio of V5+ to V4+ is about 1.41:1 according to the area ratio of their peaks, implying that ∼41.5% V4+ exists in the V2Ox film layer. The V4+ ions in V2Ox film could result in the enhancement of conductivity of the HTL,51 which facilitates the transport and collection of charge carrier in the PSC. EDS can qualitatively and quantitatively analyze all elements of the sample. The V2Ox solution is spin-coated on the polished monocrystalline silicon wafer rather than the ITO coated glass. The reason is that wafers have a lower roughness compared with the ITO film surface, which helps observe clearly the cross-section image of V2Ox film. As shown in Fig. 1b–d, the cross-section FESEM image together with vanadium elemental mapping and EDS spectrum are performed on V2Ox film based on monocrystalline silicon. The signals of V content of V2Ox film material were clearly observed. Moreover, it is important for us to point out that peaks of 2p1/2 and 2p3/2 coral electron are also clearly identified at 524.9 and 517.5 eV respectively in the XPS spectrum of the V2Ox film.
Fig. 2a and b show the schematic illustration and associated cross-section FESEM image of the prepared inverted PHJ PSC device with the structure of ITO/V2Ox/PEDOT:PSS/CH3NH3PbI3−xClx/PCBM/Ag. The double-decked V2Ox/PEDOT:PSS thin film (∼40 nm) is used as the HTL on the ITO bottom electrode (∼200 nm) of PSC device. CH3NH3PbI3−xClx film (∼250 nm) is chosen as photoactive layer, PCBM film (∼45 nm) as ETL and Ag film (∼150 nm) as top electrode. The energy level diagram corresponding to each layer of the PSC has been shown in Fig. 2c. As shown in Fig. S1,† the WF of V2Ox films are examined by UPS, and related values of ITO, PEDOT:PSS, PCBM and Ag are also given in previous studies.52 The WF of V2Ox (4.74 eV) is lower than that of PEDOT:PSS (5.10 eV),39 which could lead to the rise in short-circuit current density (JSC), enhancement the extraction of the charge carriers from the absorption layer and reduction the carriers recombination.
Fig. 2 The cross-section FESEM image (a), the schematic illustration (b) and the energy level diagram (c) of the PSC device with double-decked V2Ox/PEDOT:PSS film. |
In order to analyze the effect of different HTL films on the crystallization of CH3NH3PbI3−xClx thin films, we have measured the FESEM images of various HTL films and perovskite thin films based on HTL films. The surface FESEM images of V2Ox, PEDOT:PSS and V2Ox/PEDOT:PSS HTL films based on ITO coated glasses are shown in Fig. 3a–c, respectively. It is found that some particles with different sizes (the diameter ranges from 10 nm to 30 mm) are presented on surface of the V2Ox film. The surfaces of ITO/PEDOT:PSS and ITO/V2Ox/PEDOT:PSS films are more smooth than that of V2Ox film, which will be more conducive to the growth of CH3NH3PbI3−xClx films. The AFM images of V2Ox, PEDOT:PSS and V2Ox/PEDOT:PSS HTL films are shown in Fig. S2a–c.† The surface roughness (root-mean-square, RMS) values of the V2Ox, PEDOT:PSS and the V2Ox/PEDOT:PSS HTL films are ∼5.7 nm, ∼3.3 nm and ∼2.5 nm, respectively. Compared with conventional PEDOT:PSS films, the V2Ox/PEDOT:PSS film has a lower roughness. The roughness of the HTL film has a great influence on the morphology of perovskite films. Fig. 3d–f show surface FESEM images of CH3NH3PbI3−xClx thin films based on ITO/V2Ox, ITO/PEDOT:PSS and ITO/V2Ox/PEDOT:PSS films respectively. The V2Ox film with different sizes of particles might be detrimental to the formation of crystal nucleus sites and the growth of crystalline grains, resulting in larger pores (the diameter of pores ranges from 50 nm to 300 mm) on the perovskite film surface based on ITO/V2Ox. On the contrary, the pores of perovskite film based on ITO/PEDOT:PSS or ITO/V2Ox/PEDOT:PSS are fewer and smaller, with the diameter of less than 50 nm. Furthermore, compared with the other two perovskite films, the film based on ITO/V2Ox/PEDOT:PSS shows a larger crystal grains and more uniform surface topography, which results from the smoother V2Ox/PEDOT:PSS HTL film (Fig. S2†). This is consistent with the results presented in the XRD pattern (Fig. 4a). The XRD analysis of CH3NH3PbI3−xClx films shows diffraction peaks at 14.22°, 28.56°, and 43.29°, corresponding to (110), (220), and (330) planes, respectively. The lattice parameters of CH3NH3PbI3−xClx films with tetragonal perovskite structure are a = 8.825 Å, b = 8.835 Å and c = 11.24 Å, similar to that of CH3NH3PbI3 previously reported.10,44 Probably, the weak diffraction peaks of PbI2 appear at 12.77° and 25.71°, because CH3NH3PbI3−xClx film is decomposed into a little PbI2 under the condition of prolonged annealing. Obviously, compared with other two perovskite films, CH3NH3PbI3−xClx thin film with double-decked V2Ox/PEDOT:PSS film has a better crystallinity, which is in alignment with the FESEM images (Fig. 3d–f). The UV/Vis absorption spectra of the CH3NH3PbI3−xClx films spin-coated on the different HTLs are shown in Fig. 4b. The perovskite film with double-decked V2Ox/PEDOT:PSS layer has a stronger absorption within the ranges of 300–800 nm, compared with other two perovskite films. In order to further confirm performances of the HTLs serving as charge acceptors within the PSCs, steady-state PL measurements were carried out to investigate the quenching of perovskite emission. The quenching of the PL emission by the V2Ox, PEDOT:PSS and V2Ox/PEDOT:PSS layers can be clearly observed in Fig. 4c. The steady-state PL response clearly shows that the CH3NH3PbI3−xClx films with HTLs appear a PL intensity peak at about 780 nm. It should be noted that the PL intensity of CH3NH3PbI3−xClx film with double-decked V2Ox/PEDOT:PSS layer is the lowest. This indicates that the double-decked V2Ox/PEDOT:PSS film plays an important role in quenching recombination channels of electrons and holes in PSC devices.
To further understand the mechanism of performance improvement of PSCs with the double-decked V2Ox/PEDOT:PSS HTL, the J–V curves (Fig. 5b) of three devices are recorded in the dark conditions. Dark current measurement is an effective method of evaluating the recombination of free carriers and charge carrier loss in the leakage pathways.55 It can be shown that the double-decked V2Ox/PEDOT:PSS and PEDOT:PSS/V2Ox could simultaneously prevent the leakage current under the condition of reverse bias and improve the current injection under the forward bias. Obviously, the smallest leakage current density and the largest rectification ratio are presented in the dark J–V curve of the device with double-decked V2Ox/PEDOT:PSS at reverse-biased region, indicating a desired diode characteristics.56 EIS measurements are performed to analyze the interfacial charge transfer process of devices. The Nyquist plots of three devices with different HTLs are shown in Fig. 5c. The frequency range measured is from 106 to 1 Hz with AC amplitude of 10 mV at 0.84 V bias. Each impedance spectra is simulated through an equivalent circuit, forming a semicircle. The photovoltaic parameters of the devices are shown in Table 1, including series resistance (Rs), parallel resistance (Rp) and capacitance (C). It is found that C is similar among three devices with different HTLs while their Rp are changed regularly. The resistance of charge transport of the device with double-decked V2Ox/PEDOT:PSS film is the lowest. This indicates that charge transport rate of the device with double-decked V2Ox/PEDOT:PSS HTL film is the biggest among devices in this study.
Devices | Rs (Ω) | Rp (kΩ) | C (nF) |
---|---|---|---|
With PEDOT:PSS | 39.91 | 18.87 | 6.25 |
With V2Ox/PEDOT:PSS | 43.17 | 13.08 | 7.36 |
With PEDOT:PSS/V2Ox | 336.89 | 43.17 | 7.61 |
The valence state of the vanadium element in the vanadium oxide has exerted a great influence on the conductivity of the HTL thin film and photoelectric properties of the PSC device. In our study, we change the valence of vanadium in the V2Ox by adjusting the molar ratio (1:20, 1:40, 1:60, 1:80 and 1:100) of V2O5 to H2O2. The photograph of various V2Ox solutions is shown in Fig. 6a. As the proportion of H2O2 increases, the color of the V2Ox solution gradually becomes light. The contents of V4+ and V4+ of the V2Ox thin film measured by XPS are shown in Table 2. The content of V4+ increases with the ratio of H2O2, resulting in a higher conductivity of the double-decked V2Ox/PEDOT:PSS HTL film. As shown in Fig. 6b–e, the mean and standard deviations of the VOC, JSC, FF and PCE of PSC devices with different molar ratios of H2O2 to V2O5 are calculated. It is found that the JSC increases with molar ratio of H2O2 to V2O5. The conductivity of the double-decked V2Ox/PEDOT:PSS HTL film improves with the increase of V4+, thus the JSC of the device increases. However, the VOC, FF and PCE show a trend—increase and then decline. Possibly, the decline of V5+ results in less doping and more defects of V2Ox thin film, as well as a lower performance of device. The best-performance (Fig. 6f) and high-reproducibility device is achieved when the molar ratio of V2O5 to H2O2 is 1:60, namely, the content of V4+ is 41.5%.
V element | Molar ratios of V2O5 to H2O2 | ||||
---|---|---|---|---|---|
1:20 | 1:40 | 1:60 | 1:80 | 1:100 | |
V4+ | 33.52% | 38.13% | 41.47% | 43.97% | 45.38% |
V5+ | 66.48% | 61.87% | 58.53% | 56.03% | 54.62% |
The concentration of V2Ox solution has a great influence on the thickness and uniformity of the double-decked V2Ox/PEDOT:PSS HTL film. Therefore, we prepare V2Ox solutions with different concentration gradients (0.01, 0.02, 0.03, 0.04 and 0.05 M). The J–V characteristics of PSC based on pristine PEDOT:PSS and double-decked V2Ox/PEDOT:PSS HTL film with varied concentration of V2Ox solution are shown in Fig. 7a. The Table 3 shows the key performance parameters of PSCs, including VOC, JSC, FF and PCE. The best performance of device is achieved under the concentration of 0.03 M of V2Ox solutions. With the increase of concentration of the V2Ox solution, all performance parameters of devices show a trend, that is, increase first and then decrease, except JSC. The reason why JSC keeps rising is that a higher concentration of V2Ox solution allows the V2Ox film to have a larger contact area with the PEDOT:PSS film. The thickness of the double-decked V2Ox/PEDOT:PSS HTL film increases with concentration of V2Ox solution. On the one hand, when the concentration of V2Ox solution is very low, the V2Ox particles excessively disperse, failing to form the film. On the other hand, when the concentration of V2Ox solution gets very high, the film has a higher roughness. Moreover, there is a large barrier to extraction through the metal oxide valence band, because the V2Ox/PEDOT:PSS layer is too thick to allow the tunnelling of charges. There is no doubt that these two aspects of the factors are not conducive to preparing high-performance devices. Fig. 7b shows the IPCE spectra of the PSCs based on pristine PEDOT:PSS and double-decked V2Ox/PEDOT:PSS HTL film. Compared with the conventional AM 1.5 solar radiation spectrum,57 interestingly, the IPCE of devices based on V2Ox/PEDOT:PSS increases within a wide wavelength range between 500 and 700 nm, indicating that the devices with double-decked V2Ox/PEDOT:PSS HTL can absorb more solar energy and convert it into electrical energy. In particular, the performance of the device with 0.03 M V2Ox is the best among devices.
Devices | VOC (V) | JSC (mA cm−2) | FF | PCE (%) |
---|---|---|---|---|
Reference | 0.92(0.91 ± 0.03) | 22.25(21.26 ± 1.07) | 0.72(0.67 ± 0.07) | 13.56(11.85 ± 1.81) |
0.01 M | 0.93(0.92 ± 0.02) | 22.15(21.23 ± 0.98) | 0.72(0.68 ± 0.06) | 14.95 (13.53 ± 1.75) |
0.02 M | 0.94(0.93 ± 0.02) | 22.19(21.57 ± 0.75) | 0.73(0.71 ± 0.03) | 15.32(14.17 ± 1.17) |
0.03 M | 0.94(0.93 ± 0.01) | 22.41(21.96 ± 0.51) | 0.75(0.74 ± 0.02) | 15.86(14.97 ± 0.91) |
0.04 M | 0.93(0.92 ± 0.01) | 22.63(21.97 ± 0.89) | 0.74(0.73 ± 0.03) | 15.67(14.75 ± 0.99) |
0.05 M | 0.93(0.91 ± 0.04) | 23.12(21.99 ± 1.19) | 0.74(0.66 ± 0.09) | 15.18(13.98 ± 1.69) |
The best performance of PSC device is achieved by controlling the optimal molar ratio of V2O5 to H2O2 and the concentration of the V2Ox solution. The J–V curve and main parameters (VOC, JSC, FF and PCE) of the best-performance device with the double-decked V2Ox/PEDOT:PSS HTL film are shown in Fig. 8a. A best PCE of 15.86%, corresponding to a JSC of 22.69 mA cm−2, a VOC of 0.93 V, and a FF of 0.75, is achieved. In our study, as shown in the histograms of PCE parameters of reference devices with PEDOT:PSS HTL (30 cells) (inset) and controllable devices with the double-decked V2Ox/PEDOT:PSS HTL (120 cells) (Fig. 8b), the devices performance follows a Gaussian distribution and achieves the PCEAVE of 11.85% and 14.97% respectively. The relative standard deviations of the reference devices and devices based on the V2Ox/PEDOT:PSS are 9.8% and 4.5%, respectively, indicating that the latter shows a better reproducibility than the former.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/c7ra04414c |
This journal is © The Royal Society of Chemistry 2017 |