Paulina Sobierajskaa,
Katarzyna Zawiszaa,
Robert M. Kowalski
a,
Guillaume Renaudin
b,
Jean-Marie Nedelec
b,
Jan Zienkiewicza and
Rafal J. Wiglusz
*a
aInstitute of Low Temperature and Structure Research, PAS, Okolna 2, 50-422 Wroclaw, Poland. E-mail: R.Wiglusz@int.pan.wroc.pl; Fax: +48 071 3441029; Tel: +48 071 3954159
bUniversité Clermont Auvergne, CNRS, SIGMA Clermont, ICCF, F-63000 Clermont-Ferrand, France
First published on 9th June 2017
The nano-biphasic calcium phosphate co-doped with 1 mol% Er3+ and 5 mol% Yb3+ ions was prepared using Pechini's technique. The preparation of the biphasic calcium phosphate showed the removal of fluorine ions from the matrix. The structural properties and morphology of the particles were studied by means of XRD (X-ray powder diffraction), TEM (Transmission Electron Microscopy), and SEM (Scanning Electron Microscopy) techniques. The spectroscopic properties of Ca10(PO4)6F2/Ca3(PO4)2:Er3+,Yb3+ nano-biphasic calcium phosphate were investigated in detail using emission spectra, power dependence and emission kinetics. This material demonstrated intense green up-conversion depending on laser power. Additionally, the luminescence lifetimes for Er3+ ions were calculated from the measured decays. Power dependence of the green and red emissions was found to result from a temperature increase of nano-biphasic calcium phosphate that opens potential applications in theranostics.
Presently, fluorine ions (F−) are the most frequently used supplement in hydroxyapatite, which improves its physicochemical properties such as solubility, thermal stability, crystallinity and resistance to acid corrosion.5–8 Furthermore, it enhances bone growth, osseointegration and mineralization.9,10 The F− ion is a microelement present in human enamel and possesses inhibiting properties to bacterial metabolism.11–13 Due to the absence of OH− ions that are luminescence quenching centers, fluorapatite lattice is expected to be a more suitable matrix for luminescence applications.14 The fluorine ion is smaller (1.28 Å) compared to the hydroxyl ion (1.37 Å), so F− ions can fill more closely the unit cell resulting in smaller cell volume.15
The fluorapatite (Ca10(PO4)6F2 – hereafter FAp) crystallizes in hexagonal space group P63/m and contains ten calcium cations located in two nonequivalent sites – four Ca(1) ions with three-fold C3 symmetry surrounded by nine oxygen atoms, and six Ca(2) ions with Cs symmetry coordinated by six oxygen atoms and one fluoride atom. Rare earth ions could substitute calcium in both sites.16 This compound has been used as a host lattice for luminescent ions such as europium,16 neodymium,17 praseodymium,18 co-doped by ytterbium and holmium19 amongst others. It is well known that fluorine ions release from lattice during material thermal treatment, especially when material is highly carbonated.20,21
The β-TCP crystallizes in the rhombohedral space group Rc and it is isostructural to the natural mineral whitlockite: Ca18.19Mg1.17H1.62(PO4)14. The calcium ions are present in five different crystallographic sites. Four sites Ca(1), Ca(2), Ca(3) and Ca(5) are wholly occupied, but the Ca(4) position is half occupied in a statistical way. The Ca(1), Ca(2), Ca(3) and Ca(5) are coordinated respectively with seven, eight, eight, and six oxygen atoms. Ca(4) is threefold coordinated implying weak bonding and the formation of vacancy.22,23 The solubility activity product of β-TCP is higher than hydroxyapatite causing faster bone growth and integration with bone tissue.24,25 The advantageous role of the β-Ca3(PO4)2 is related to facilitate the bone-formation on their surface by influence of the processes connected with attaching, proliferation as well as migration of the bone cells.26 Therefore, the enhancement of biodegradation relies on the preparation of mixtures or composites containing both phases of phosphates. There are some studies concerning β-TCP co-doped with lanthanides ions (the β-TCP:Er3+/Yb3+) that consider the in vivo bioimaging under IR excitation (upconversion process)27 as well as doped with Eu3+
28 and Eu2+
29 ions for light industry applications amongst others.25,30–32
The most of the bio-applications require nanosized materials, but the number of current studies on luminescent apatite nanoparticles is very limited. Calcium phosphates doped with luminescent ions are studied as inorganic labels aimed at fluorescence imaging, which is one of the most important techniques used in diagnostic applications.19,33 The doped and co-doped apatites, in comparison with fluorescence organic labels, are more resistant to aggressive factors such as photodegradation, high temperature, or oxidation process, the emission are characterized by narrow and intense bands, high fluorescence quantum yield, long decay times, therefore these materials are promising for bio-detection applications. The excitation by NIR radiation lead to deeper tissue penetration due to “the optical transparency window” of biological tissue (700–1100 nm).19,33 The up-converting nanoparticles (UCNP) are the most important material devoted to this purpose owing to their excitation at NIR range of electromagnetic radiation. In the up-conversion process, two or more low-energy photons (in NIR range) are converted into a high-energy photon (in UV-VIS region), which is founded on sequential absorption and energy transfer between doping ions (e.g. Er3+/Yb3+).34,35
In the paper, there is presented the results concerning biphasic calcium phosphate of fluorapatite (FAp) and β-tricalcium phosphate (β-TCP) co-doped with Er3+ and Yb3+ ions obtained using the sol–gel synthesis. First of all, it is very important aspect of biomaterial preparation, in the case of the biphasic materials, to obtain the difference of solubility between them (β-TCP being far more soluble than FAp). The mixture of the two compounds known as the Biphasic Calcium Phosphate (BCP) are highly desirable for bone substitutes and bone cement applications. Mixing of both phosphates contributes to better cellular response to the applied material due to better integration with a tissue.36,37
Secondly, upconversion luminescent nanoparticles (UCNP) with the anti-Stokes emission have been paid attention in the field of biomedicine as theranostic agents.38 The emission and excitation of UCNPs is located in the optical window of biological tissue what minimize the overheating effect from the excitation irradiation at 980 nm the biological markers.39
Therefore, the aim of proposed research was to obtain the bioactive materials with controlled biodegradability, intended for the future theranostic applications, especially within the cranial and facial bones.
The modified Pechini's method combines the advantages of sol–gel as well as thermal decomposition techniques. Such method requires using organic substrates such ethylene glycol and citric acid forming polymer–metal ions resins. The modified Pechini's method offers a chemically homogeneous product with high purity. However, in the case of calcium phosphates the high annealing temperature about 700 °C, in order to remove any organic components, is the reason to obtain the multiphasic materials.
![]() | (1) |
The emission was observed using a set-up consisting of a grating spectrograph Princeton Instrument Acton SP2500 and a streak camera Hamamatsu C5680. The power dependence of the up-conversion emission intensity was measured using a laser diode Apollo Instruments F4-980-6 emitting continuous 980 nm line on powders. The data were fitted according to the following formula:
IUPC = IinN, | (2) |
NH4+ + F− → NH4F↑ | (3) |
![]() | ||
Fig. 1 Effect of annealing temperature on the structure evolution of the Ca10(PO4)6F2/Ca3(PO4)2 co-doped with 1 mol% Er3+ and 5 mol% Yb3+. |
The obtained powders were ascribed to the FAp crystallizing in the hexagonal structure with space group P63/m (ICSD 9444) and to rhombohedral β-TCP with Rc (ICSD 97500), respectively. Over the entire temperature range, phase decomposition of the obtained materials was noted by XRD analysis. However, the FAp and the β-TCP phases were observed at all annealing temperatures. Moreover, up to 900 °C, the traces of the REPO4 (where RE – Er3+, Yb3+) were identified, but these extra phases were not found at 1000 °C. As can be seen, with the increase of temperature treatment, the amount of the FAp phase was reduced in favour of the β-TCP phase. At temperature of 1000 °C, much more tricalcium phosphate was identified than fluorapatite in the biphasic calcium phosphate studied herein.
Since the goal of the studies was to obtain the Ca10(PO4)6F2/Ca3(PO4)2 nano-biphasic calcium phosphate, in accordance with the XRD analysis, for further characterization, the sample heat-treated at 1000 °C was chosen.
The β-tricalcium phosphate possesses five different Ca2+ crystallographic sites and the fluorapatite has two non-equivalent Ca2+ sites, Ca(1) coordinated by nine oxygen atoms and Ca(2) coordinated by six oxygen atoms and one fluoride ion. The ionic radii of Er3+ and Yb3+ cations are quite similar to calcium ion thereupon, it can be predicted that these cations will enter most of the Ca2+ sites in both the fluorapatite and the β-TCP host lattices.
The visualisation of the fluorapatite (up) and the β-tricalcium phosphate (bottom) unit cells and the coordination polyhedra of Ca2+ cations are presented in Fig. 2.
![]() | ||
Fig. 2 The projection of the FAp (top) and β-TCP (bottom) unit cell with the indication of the coordination polyhedral. |
The structural refinement was done by using the Maud program version 2.6840,41 and based on the fluorapatite crystals with hexagonal structure and β-tricalcium phosphate crystal using a better approximation as well as indexing of the Crystallographic Information File (CIF). The quality of structural refinement was checked by R-values (Rw, Rwnb, Rall, Rnb and σ) since these numbers are easy to detect being consistent with a hexagonal structure of fluorapatite and a rhombohedral structure of tricalcium phosphate. Furthermore, a difference in plotting observed and calculated patterns is the best way to judge the success of Rietveld refinement. The parameters with additional functions were applied to find a structural refinement with better quality and reliability. The conformation of the hexagonal and the rhombohedral phase formation were affirmed by the obtained results. Fig. 3 shows a good agreement between the observed XRD pattern and the theoretical fit which indicates the validity of the Rietveld refinement method as illustrated by the small differences near to zero in the intensity scale in the line (YObs − YCalc). More details regarding Rietveld refinement are displayed in Table 1.
According to the HRTEM study, the primary size and morphology evaluation of the 1 mol% Er3+, 5 mol% Yb3+ doped Ca10(PO4)6F2/Ca3(PO4)2 particles were explored by means of transmission electron microscopy (TEM) and was found to be around 90 nm in the case of the 1000 °C temperature treatment (see Fig. 4). The spherical particles as well as agglomerated irregular grains were observed. The broad distribution of the primary size is characteristic of all materials where high temperature thermal treatment has been involved.
![]() | ||
Fig. 4 (a) TEM and (b, c) SAED images of the Ca10(PO4)6F2/Ca3(PO4)2 biphasic calcium phosphate doped with 1 mol% Er3+ and 5 mol% Yb3+ prepared at 1000 °C. |
In accordance with analysis of the SAED (Selected Area Electron Diffraction) images (see Fig. 4b and c) this points to the presence of well-developed spotty rings confirming a high level of material crystallization. Moreover, the obtained sample calcined at 1000 °C shows the SAED spots patterns with the clear diffraction patterns indicating strong development of rhombohedral Ca3(PO4)2 (see Fig. 4b) and hexagonal Ca10(PO4)6F2 (see Fig. 4c) phases. These SAED analyses confirmed the formation of both structures and are in agreement with the XRD results.
In order to confirm the content of particular elements in the material, the EDX (Fig. 5) as well as ICP techniques were employed. The element maps were drawn up by the SEM-EDS measurement to check the incorporation regularity of the cations into the lattice (Fig. 6).
![]() | ||
Fig. 6 SEM-EDS elemental maps of the Ca10(PO4)6F2/Ca3(PO4)2 biphasic calcium phosphate co-doped with 1 mol% Er3+ and 5 mol% Yb3+ prepared at 1000 °C. |
The results confirm the stoichiometric contents and regular substitution of cations in the material. The SEM-EDS analysis was performed for all samples to verify the content of fluorine ions. The process of defluoridation was observed depending on the annealing temperature (see Fig. 5). The fluorapatite component released fluoride during heat-treatment, particularly above 1000 °C. This may be caused by removal of NH4F compound due to its low decomposition temperature (∼100 °C). Another reason for lower fluorine content could be connected with the removal of carbon dioxide, which exists in several forms depending on the temperature. Above 800 °C it flies in the form of CO3F.20 Since the sample was prepared by the sol–gel method using a large amount of citric acid and ethylene glycol, there is plenty of carbon. Moreover, the sol–gel preparation showed the removal of fluorine ions from apatite materials. Such phenomenon could be valuable in the development of bioactive phosphates preparation for a controlling of the fluoride ion concentration, especially for dental managements. It is worth pointing out that excessive concentration of the fluoride ions could be toxic and leading to the dental fluorosis characterized by the hypo-mineralization of tooth enamel.11 Moreover, the fluoride ions used as a substitution in the hydroxyapatite improve its physicochemical properties thus promote osteoblastic activities in terms of cell proliferation and differentiation as well as bone mineralization.10 The fluoride ions doped hydroxyapatite prevent, reduce and control dental caries.44
The up-conversion emission transitions can be identified as a group of lines in the green spectral range of 520–575 nm (19231–17
391 cm−1) connected with the 2H11/2 → 4I15/2 and the 4S3/2 → 4I15/2 electronic transitions, and in the red region of 635–700 nm (15
748–14
286 cm−1), attributed to the 4F9/2 → 4I15/2 transition. These peaks are relatively broad and not resolved into particular Stark components. An occupation of different crystallographic sites by Er3+ and Yb3+ ions which thereupon create an overlap of emission lines from respective sites could be the reason for broadening of emission transitions.
Moreover, further reasons could explain such behaviour such as different oxidation states of dopants or structural defects, so-called charge compensation mechanisms and their heterogeneous distribution in nanomaterials as well as small particle size resulting into larger surface area.45,46 It is well known that the 2H11/2 → 4I15/2 transition changes drastically in comparison with 4S3/2 → 4I15/2 under the dependence of laser power. This is related to the Er3+ ions as a temperature sensor in this spectral region.47 This could be confirmed by the streak camera images taken at 300 K as shown in Fig. 8 (left). Moreover, it could be noted that the intensity of the green emission of Er3+ ions increased in relation to red emission with the increasing laser power. The analysis of the integrated intensity ratio between green and red transitions could be considered as an indirect method for estimating the efficiency of the up-conversion process (green-to-red ratio GRR) (see Fig. 8 (right)). The GRR ratio depends directly on occupied point symmetry and the closest surrounding of emitting ions in the crystal field as well as excitation power related to the thermal effects influencing population of electronic states.
Furthermore, it is noteworthy that laser power significantly affects the relative intensity of the 2H11/2 → 4I15/2 and the 4S3/2 → 4I15/2 causing self-heating of the sample. This is related to the Boltzmann's distribution populated by both overlapping energy levels:
![]() | (4) |
The pump power dependence of both 2H11/2, 4S3/2 → 4I15/2 and 4F9/2 → 4I15/2 transitions were investigated for the Ca10(PO4)6F2/Ca3(PO4)2 biphasic calcium phosphate co-doped with 1 mol% Er3+ and 5 mol% Yb3+ prepared at 1000 °C (see Fig. 9). The up-conversion emission results were fitted giving slope values of the linear function around 1 (1.4) for the red band and close to 2 (1.9) for the green band confirming the involvement of 2 photons in green emission. It was observed an increase in the GRR with LD power due to the higher population of 2H11/2 → 4I15/2 (so-called thermalization process).
![]() | ||
Fig. 9 Power dependence of the Ca10(PO4)6F2/Ca3(PO4)2 biphasic calcium phosphate co-doped with 1 mol% Er3+ and 5 mol% Yb3+ prepared at 1000 °C. |
The spectral behavior of the UC processes as well as the dynamics of the signal indicate that involving Er3+ and Yb3+ ions is the mechanism for emissions at 523, 548 and 665 nm.
In the literature, three mechanisms for the up-conversion emission were proposed: the APTE effect called ETU (energy transfer up-conversion), excited state absorption (ESA) and photon avalanche (PA). Moreover, it is difficult to distinguish these processes directly due to the quadratic power dependence.
The schematic and simplified energy level diagram presenting the most important accompanying and contributing processes to the up-conversion emission in the Er3+ and Yb3+ ions co-doped Ca10(PO4)6F2/Ca3(PO4)2 (see Fig. 10). The NIR absorption of photons through the Yb3+ and Er3+ electrons directly from the ground states 2F7/2 and 4I15/2 are excited to the 2F5/2 and 4I11/2 levels by GSA processes. First, the absorbed photon shifted electrons were formed from 4I11/2 level to the 4F7/2 by excited state absorption (ESA). Next, the energy was absorbed by Yb3+ ions and the electrons could be moved simultaneously to the 4F7/2 level of Er3+ ion by ETU (energy transfer up-conversion) as well as the 4I11/2 level of the Er3+ ion by ET (energy transfer) processes. These processes require the participation of at least two photons. After that, the electrons from the 4F7/2 level relaxed very fast non-radiatively to the 2H11/2 and 4S3/2 levels through multiphonon relaxation process (MPR) or farther to 4F9/2 level by cross relaxation (CR) and beyond these levels, green or red emission may occur up to the 4I15/2 ground state. The CR depends on the ion concentration in the matrix as well and is sensitive to laser-power. Several highly probable processes of the CR may occur:
(1) CR1: (4F9/2) → (4S3/2, 4I9/2); |
(2) CR2: (4F9/2) → (4F7/2, 4I11/2); |
(3) CR3: (4I9/2) → (4S3/2, 4I13/2). |
![]() | ||
Fig. 10 Simplified energy level scheme presenting up-conversion the Ca10(PO4)6F2/Ca3(PO4)2 biphasic calcium phosphate. |
It can be noticed that the efficiency of the up-conversion process between Yb3+ and Er3+ ions located in biphasic phosphate was demonstrated with the increase of excitation power. A strong power dependence of the green and red emissions was found to be a result of temperature increase of nano-biphasic phosphate which show the potential prospect of that kind of ceramic in temperature-sensing applications. The luminescence nanothermometry exploits the relation between temperature and luminescence properties to achieve thermal sensing from the spectral analysis of the measured material. In case of Er3+ and Yb3+ pairs of ions it is possible to monitor the temperature of the particle by analyzing the emission spectra due to the 4S3/2 state is a metastable and the population of 2H11/2 increases via its Boltzmann population (see eqn (4)). The relation between that states is shown as FIR power dependence (see Fig. 8, inset) which presents how using the relative emission intensity can determine the temperature of the nanocrystal. That phenomenon makes the Ca10(PO4)6F2/Ca3(PO4)2:Er3+,Yb3+ an attractive composite for use in nanothermometry.
The luminescence decays of the green and red emissions showed a double-exponential character and exhibited long (37.06–21.81 μs) and short (6.46–8.12 μs) components, suggesting the presence of more than one emitting centre (see Fig. 11). The double-exponential behaviour may be explained by various possible mechanisms. First of all, it could be related to the effects on particle surfaces. The ions located close to the surface are exposed to changes in the local environment and exhibit shorter luminescence times than these closer to particle cores with/displaying longer luminescence decays. Moreover, the dopant could be located in two different phases of the obtained sample which showed a significant contribution of the β-TCP phase at 1000 °C. In fact, in many up-converting materials, the radiative decay times of both green and red transitions are usually a few hundred microseconds in low concentrated samples and dozens of microseconds in highly concentrated samples.
![]() | ||
Fig. 11 Luminescence decay curves of the Ca10(PO4)6F2/Ca3(PO4)2 biphasic calcium phosphate co-doped with 1 mol% Er3+ and 5 mol% Yb3+ prepared at 1000 °C, under pulsed laser excitation at 980 nm. |
A biphasic calcium phosphate has been chosen as a material for implantology to improve dissolution characteristics imparted by the addition of β-tricalcium phosphate. The β-TCP phase undergoes faster resorption than FAp, allowing the precipitation of apatites. The choice of fluorapatite is reasonable due to more thermally stable and higher crystallinity than hydroxyapatite, what is also significant in cement production for implantology. The Ca10(PO4)6F2 and Ca3(PO4)2 materials from different stable phases and the bioactivity as well as biodegradation of a biphasic phosphate containing both phases depends strongly on the variation of the ratio of FAp/β-TCP.
It has been shown that the interplay of the intensity between transitions of the 2H11/2 → 4I15/2 and the 4S3/2 → 4I15/2 changes during sample heating induced by different laser power levels suggesting possible applications of this material in nanothermometry. The analysis of the GRR ratio showed that increasing the GRR with laser power was attributed to the thermalization process resulting in a higher population of the 2H11/2 → 4I15/2 transition.
The luminescence decays were double-exponential and exhibited short and long decay components. The double exponential behavior is related by the presence of surface effects where the Er3+ ions are located at the surface and are more sensitive to the local environment as well as exhibit longer luminescence lifetimes. Moreover, the dopants are located in two different phases of the obtained sample with a significant contribution of the β-TCP phase.
This journal is © The Royal Society of Chemistry 2017 |