K. H.
Sizeland
ab,
H. C.
Wells
b,
S. J. R.
Kelly
b,
R. L.
Edmonds
c,
N. M.
Kirby
a,
A.
Hawley
a,
S. T.
Mudie
a,
T. M.
Ryan
a and
R. G.
Haverkamp
*b
aAustralian Synchrotron, 800 Blackburn Road, Clayton, Melbourne, Australia
bSchool of Engineering and Advanced Technology, Massey University, Palmerston North, New Zealand. E-mail: r.haverkamp@massey.ac.nz
cLeather and Shoe Research Association, Palmerston North, New Zealand
First published on 21st August 2017
Water interacts with collagen to alter the structure at the fibrillar scale and therefore the mechanical properties of collagen. Humectants or moisturizers also alter the mechanical properties and fibril structure. The nature of these interactions and relationship between the different additives is not well understood. Changes in collagen D-spacing in leather were measured by synchrotron based small angle X-ray scattering in samples stored at various relative humidities and treated with lanolin, fatliquor, urea, proline or paraffin. The D-spacing increased with rising humidity and with increasing lanolin or fatliquor content, but not with treatment with urea, proline or paraffin. Strength increased with the addition of lanolin. Lanolin and fatliquor were shown to act as humectants whereas the other components did not act in this way. The Hofmeister effect is shown not to be a factor in the change in D-spacing, since samples treated with either proline or urea exhibited the same behavior. Different agents used in leather treatment and skin care function by different mechanisms, with collagen water retention being important for some additives but not others.
Type I collagen has a complex hierarchical structure, and like all proteins this structure is mediated by hydrogen bonds. Type I collagen is a fibrillar protein composed of alpha helical polypeptide chains with a left-hand twist. It contains a repeating glycine–X-Y amino acid sequence where a high proportion of X and Y positions are occupied by the amino acids proline and hydroxyproline.1,2 Three collagen molecules twist together in a right-hand manner to form a triple helix, or tropocollagen. Hydrogen bonds between side-chains stabilize the tropocollagen tertiary structure along with some covalent crosslinks. Collagen fibrils are assembled from multiples of five tropocollagens. Interchain hydrogen bonds are present as either direct or water-mediated bonds.3 The staggering of the tropocollagen in collagen fibrils produces bands, with thinner parts containing a multiple of four tropocollagens and thicker parts a multiple of five tropocollagens. This results in a d-periodicity, with characteristic D-spacing that is visible in transmission electron microscopy, atomic force microscopy and X-ray and neutron diffraction.4–6
Skin and other tissues are highly hydrated. Although collagen is hydrophilic and strongly associates with water, the high water content in the dermis has been attributed to the hydrophilic extracellular glycosaminoglycans also present.7 Water modifies the properties of collagen-based tissues, imparting additional suppleness and elasticity to the materials.8 Water also affects the mechanical properties of processed materials such as leather and surgical scaffolds, increasing their flexibility.9
Water has been known, from the early days of collagen structure investigation, to affect the X-ray diffraction pattern of collagen.10 The d-periodicity of collagen decreases as collagen is dehydrated.11,12 This change in the structure of collagen may be a contributing factor in the change in its physical properties.
Suppleness may also be achieved by the application of other components. In leather “fatliquors” (usually mixtures containing polyols) are added to improve the strength and haptic properties of leather.13 Many dermatology products are used to improve the suppleness of skin. Moisturizers or emollients for dermatology may act as occlusive moisturizers (containing paraffin, petroleum jelly, cocoa butter, silicones and lanolin14 or a range of other fatty alcohols or fatty acids), blocking the evaporation of water, or as humectants (containing urea,15,16 glycerol, lactic acid, glycolic acid or salicylic acid),17 causing water retention.
Fatliquor and lanolin have both been shown to increase the D-spacing of leather18 approximately in proportion to the amount present while increasing the tear resistance.19 The addition of fatliquor increases extensibility and tear strength of leather.12
Here we investigate the mechanism by which water, in combination with moisturizing agents such as fatliquor and urea, modifies the properties of collagen by observing the changes in the collagen fibril structure.
Ovine pelts were obtained from 5 month-old, early season, New Zealand Romney-cross lambs. The leather was generated using conventional beamhouse and tanning processes. Specifically, the skins were depilated using a caustic treatment comprising sodium sulfide and calcium hydroxide. The leather was then rotated in a drum for 16 h at 20 °C in a 1.2% sodium sulfide solution to remove any residual keratinaceous material. The skins were next washed to remove the lime and treated with 0.1% of a commercial bate enzyme (Tanzyme, Tryptec Biochemicals, Ltd.). They were then pickled in a 2% sulfuric acid and 10% sodium chloride solution. The pickled pelts were pre-tanned using oxazolidine, degreased with an aqueous surfactant, and tanned using chromium sulfate. Finally, a 3% vegetable tanning material (mimosa, Tanac, Brazil) was used to re-tan the resulting “wet blue”.
In conventional beamhouse processing, fatliquors are added at this stage to the wet blue pelts prior to fixing with 0.5% formic acid, washing, drying and mechanical softening. The standard fatliquored samples in this study were made using 0–10% Lipsol EHF. For the other samples in this study, the fatliquor was replaced with urea or L-proline at concentrations of 4% and 7.2% by weight of wet leather, or the fatliquor was replaced with 0–10% lanolin by weight of wet leather.
The fatliquor content of samples processed with offerings of 0–10% lipsol EHF and 0–10% lanolin was determined using the standard method ISO 4048. 10 g of ground leather was extracted using at least 30 changes of dichloromethane in a Soxhlet extraction apparatus. After drying the extract in an oven at 102 °C for at least 4 h, the resulting grease was cooled in a desiccator and weighed. The percentage fat is quoted on the basis of a moisture content in the leather at 74% relative humidity (RH).
Tear strengths of the leathers were measured using standard methods.20 Samples were cut from the leather at the official sampling position (OSP).21 The samples were then conditioned by holding at a constant temperature and humidity (23 °C and 50% relative humidity) for 24 h, after which time the samples were tested on an Instron strength-testing device.
The samples for SAXS analysis were cut from the OSP21 in strips 1 × 30 mm. Each sample was mounted without tension in the X-ray beam to obtain scattering patterns through the sample's full thickness. Each data point presented here is the average of 11–17 diffraction patterns recorded every 0.25 mm through the cross-section from the grain to the corium except the sample with no additives, which is the average of six patterns. Diffraction patterns were recorded on the Australian Synchrotron SAXS/WAXS beamline using a high-intensity undulator source. Energy resolution of 10−4 was obtained from a cryo-cooled Si (111), double-crystal monochromator, and the beam size (FWHM focused at the sample) was 250 × 80 μm, with a total photon flux of about 2 × 1012 photons s−1. All diffraction patterns were recorded with an X-ray energy of 11 keV using a Pilatus 1 M detector with an active area of 170 × 170 mm and a sample-to-detector distance of 3371 mm. Exposure time for diffraction patterns was 1 s, and data processing was carried out using scatterBrain Analysis software (Australian Synchrotron).
D-Spacing was calculated from the position of the 6th order diffraction peak, taking the centre of a Gaussian curve fitted to the peak after subtraction of the background. Four scattering patterns were collected on each of two samples and averaged to produce one value.
Samples for SAXS analysis were maintained at controlled humidity. Untreated leather and lipsol-, lanolin-, urea-, and proline-treated leather were placed onto plastic grids in sealed containers containing one of a saturated solution of potassium acetate, sodium bromide, or sodium chloride. These yielded 22.5%, 57.6%, and 75.3% relative humidities, respectively. The samples were allowed to equilibrate at these humidities for 48 h prior to SAXS analysis. Samples were also soaked in water. These are shown in the results as “100% relative humidity” and plot them on the scale at this point, but they are saturated with water and contain free water. The samples were sealed in kapton tape prior to analysis to ensure they remained as close as possible to their humidity-equilibrated state.
Lanolin offer | Fat in wet blue |
---|---|
0% | 0.4% |
2% | 2.4% |
4% | 4.7% |
6% | 6.4% |
8% | 7.4% |
10% | 7.9% |
Lipsol EHF offer | Fat in wet blue |
---|---|
2% | 4% |
4% | 6% |
6% | 9% |
8% | 10% |
10% | 10% |
Fig. 2 Relative humidity versus D-spacing for: (a) lanolin (0% —, 2% , 4% , 6% , 8% , 10% ); (b) Lipsol EHF (0% —, 2% , 6% , 8% ). |
Fig. 3 D-Spacing with (a) lanolin or (b) Lipsol EHF fatliquor content at different relative humidities. |
However, the increase in D-spacing with humidity is affected very substantially by other treatment to which the leather has been exposed. It has previously been shown that lanolin or fatliquor increases the D-spacing of collagen.12,19 When more lanolin is present in leather, the change in D-spacing with increasing moisture content is smaller (Fig. 2 and 3). The D-spacing almost converges with that of the wet material, regardless of the amount of lanolin present. A similar trend is observed for the fatliquor Lipsol. It is possible that this effect is due to a combined effect of lanolin increasing the D-spacing and water increasing the D-spacing, such that the upper limit of D-spacing is approached. However, another possible explanation is that the D-spacing increase is due only to an increase in water, and that the lanolin or fatliquor contributes to the retention of water, so that at a given humidity more water is retained when lanolin is present. Lanolin (and fatliquors) is an amphoteric compound, having affinity to both polar and non-polar molecules, so it can facilitate water retention.
It could be argued that lanolin's oily nature contributes to increases in D-spacing rather than its amphoteric nature. To test this hypothesis, a comparison was made with the effect of a purely hydrophobic chemical, paraffin oil, on collagen D-spacing. While increases in humidity were still associated with increased D-spacing, the addition of paraffin oil did not enhance this effect, and at lower humidity it had the opposite effect, that of reducing the D-spacing (Fig. 5), perhaps due to its hydrophobic nature excluding water. This result supports the notion that it is not the lanolin directly that causes the increase in D-spacing, but rather the lanolin's water-retaining capacity that does so. So while lanolin is generally considered an occlusive agent in skin care,14,17 it appears from the observed increases in D-spacing of collagen that lanolin is a humectant.
Urea is commonly used as an ingredient in dermatology products,15,16 and it is also known to be near one end of the Hofmeister series as a denaturant of proteins.22 Denaturing protein involves the disruption of hydrogen bonds that provide structural form to the molecular backbone. It has been hypothesized that urea could act on collagen to weaken the hydrogen bonds and therefore expand the fibril structure (with an increase in D-spacing), and that this might provide an increase in fibril length and therefore expanded and smoother skin. However, the measurement of D-spacing of samples treated with urea does not confirm this hypothesis. While the D-spacing increased with increasing humidity it did not appear to increase with increasing urea content (Fig. 5), although the data here are rather limited and preliminary. Proline is at the other end of the Hofmeister series, and acts to precipitate proteins from solution.23 If this effect influences D-spacing then proline might be thought to decrease the D-spacing, but this was not observed. The lack of effect on D-spacing of both urea and proline suggests that the Hofmeister theory is not relevant to this phenomenon. Both urea and proline are hydrophobic24 and it is this property (the lack of amphoteric or polar nature) that may be the main factor leading to a lack of influence on the collagen D-spacing. This leaves unanswered, therefore, the question of why urea is a useful skin cream additive.
The tear strength of leather is increased with the addition of lanolin (Fig. 6) but this may be due to the lanolin's ability to enhance water retention, as the level of hydration of leather is known to affect the tear strength.9
These changes in D-spacing observed in collagen as a result of water content and facilitated by various additives may be related to the physical properties of leather and skin in two or more ways. An increase in D-spacing means longer collagen fibrils and an increase in length of a few percent may help to remove wrinkles in skin. However, an increase in length does not necessarily translate to a stronger or more supple material. The higher level of hydration that a higher D-spacing reflects may be the cause of the improved mechanical properties of skin and leather. Tropocollagen molecules are linked by extensive hydrogen bonds,3 and this hydrogen bonding requires hydration. A greater level of hydration may impact on this hydrogen bonding and the ability of the tropocollagen to move relative to neighbouring tropocollagens or for fibrils to move relative to other fibrils. In skin this may also be mediated by glycosaminoglycans.25
This journal is © The Royal Society of Chemistry 2017 |