Wei Chen,
Qingyun Liu,
Xixi Zhu and
Min Fu*
College of Chemical and Environmental Engineering, Shandong University of Science and Technology, Qingdao 266590, P. R. China. E-mail: fumin@sdust.edu.cn; fuminis@163.com; Fax: +86-532-80681197; Tel: +86-532-86057757
First published on 21st August 2017
Strontium ferrites/graphene (SrFe12O19/G) composites were synthesized by a facile one-step surfactant assisted hydrothermal method. The structure, magnetic properties and electromagnetic parameters of the as-prepared composites were evaluated. Uniform SrFe12O19 nanoparticles with a diameter of 60–70 nm were well distributed on the graphene. The formation of SrFe12O19 nanoparticles and the reduction of graphene oxide were accomplished simultaneously. The re-stacking of graphene sheets and the aggregation of SrFe12O19 nanoparticles were inhibited. The as-obtained composites exhibited better absorbing properties than the pristine SrFe12O19 particles due to the synergistic effect of SrFe12O19 and graphene. The minimum reflection loss (RL) of SrFe12O19/G composites with the thickness of 3 mm reached −34.8 dB at 13.6 GHz, and the effective absorption bandwidth (RL < −10 dB) was 5.7 GHz. However, the minimum RL of the SrFe12O19 particles only reached −13.5 dB, and the effective absorption bandwidth was 4.6 GHz. A possible mechanism for the enhanced absorbing performance was proposed.
As a kind of useful electromagnetic functional material, ferrites have aroused enormous research interests in many fields, with applications such as magneto-optical devices, magnetic memories, sensitive elements, catalysts, biology, absorbing materials and so on.5–11 As a typical hard magnetic material discovered in 1950s, strontium ferrite (SrFe12O19) is of great importance due to its low cost production, high saturation magnetization and good chemical stability.12
A number of different methods, including co-precipitation method,13 high temperature calcinations,14 sol–gel method15 and hydrothermal reaction followed by post-calcination,16 have been used to develop SrFe12O19 based materials. However, the preparation of SrFe12O19 often suffers from the agglomeration, which is caused by the magnetic dipole interaction between ferrite particles.17 Moreover, single component functional material cannot meet the ever-increasing demands for absorbing materials. Hence, combining SrFe12O19 with another suitable component would be a feasible way to solve the above mentioned problems.
Graphene, a single layer of carbon atoms patterned in a hexagonal lattice, has attracted worldwide attentions owing to its two dimensional structure, high specific surface area, super electronic, mechanical and thermal properties.18,19 Considering the excellent properties of graphene and SrFe12O19, SrFe12O19/graphene (SrFe12O19/G) hybrids can be very attractive for microwave absorbing applications. On one hand, graphene with planar structure provides an ideal platform for the growth of SrFe12O19, suppressing the aggregation of SrFe12O19 nanoparticles. On the other hand, SrFe12O19 nanoparticles on the surface of graphene inhibit the re-stacking of graphene. The structural stability guarantees the good electromagnetic properties.
Luo et al.20 prepared reduced graphene oxide/strontium ferrite/polyaniline (RGO/SF/PANI) composites by a three-step method. Firstly, they obtained SrFe12O19 nanoparticles by co-precipitation and post-calcination method. Secondly, they mixed SrFe12O19 nanoparticles with graphene oxide (GO) solution and obtained RGO/SrFe12O19 hybrids. Finally, in situ polymerization method was used to obtain RGO/SF/PANI composites. Zhao et al.21 synthesized RGO/SrFe12O19 nanoflakes composites by a two-step method. They separately prepared SrFe12O19 nanoflakes and RGO, and subsequently mixed them to obtain the composites. The absorption properties were also investigated. However, there are few reports focused on the construction of SrFe12O19/graphene composites by a one-step in situ method.
Herein we synthesize the SrFe12O19/G composites by a one-step hydrothermal reaction with the assistance of the surfactant. The formation of SrFe12O19 and the reduction of GO are accomplished simultaneously, which is much different from two-step method.20,21 Also, post-calcinations are not needed in our experiment, avoiding the introduction of impurities, and saving energy and time.16 Moreover, the planar structure of graphene and the use of surfactant restrain the aggregation of SrFe12O19 nanoparticles.3 In addition, the applications of pristine ferrites are limited due to large densities and narrow absorbed frequency. Graphene is light-weight and highly conductive, which offers the possibility of satisfying the ever-increasing demands for absorbing materials.22 The structure, morphology and absorbing properties of as-prepared hybrids were investigated. The minimum reflection loss (RL) of SrFe12O19/G composites at the thickness of 3 mm reached −34.8 dB at 13.6 GHz, which was much better than that of the pristine SrFe12O19 particles (−13.5 dB). It is believed that the as-synthesized composites can find applications in the microwave absorbing field.
Fig. 1 TEM images of the GO (a), SrFe12O19 particles (b), SrFe12O19/G composites (c and d), HRTEM images of the GO (e) and SrFe12O19/G composites (f). |
Fig. 1e illustrated the HRTEM image of GO and the lattice spacing of GO was 0.83 nm. Both the lattice fringes of graphene and SrFe12O19 nanoparticles were clearly observable in Fig. 1f. The lattice spacing of graphene was 0.36 nm, smaller than that of GO, indicating the removal of the oxygen-containing functional groups.1 The lattice fringe distances of about 0.26 nm and about 0.27 nm were indexed to the (114) and (107) planes of SrFe12O19, respectively. The clear lattice indicated that SrFe12O19 nanoparticles were of high crystallinity.
Graphene with planar structure provided an ideal platform for the growth of SrFe12O19 nanoparticles, and the existence of SrFe12O19 nanoparticles inhibited the re-stacking of graphene. Therefore, it was safe to deduce that the introduction of graphene overcame the poor dispersion of SrFe12O19 particles in the composites. The structural uniformity indicated the good electromagnetic properties and potential microwave absorbing applications of the SrFe12O19/G composites.
Fig. 2 showed FTIR spectra of the GO and SrFe12O19/G composites. The peaks of GO located at 3409, 1738, 1625, 1399 and 847 cm−1 were due to the vibration and deformation bands of O–H, CO stretching vibrations from carbonyl groups, CC configurable vibrations from the aromatic zooms, C–OH stretching vibrations, C–O vibrations from epoxy groups and alkoxy groups, respectively.18 However, most of the peaks related to the oxygen-containing functional groups disappeared in the FTIR spectrum of SrFe12O19/G composites (Fig. 2b), revealing that these oxygen-containing functional groups were almost removed after the hydrothermal reaction. The hydrothermal condition with ammonia provided thermal and chemical factors to reduce the GO. The peaks at 1613 cm−1 were attributed to the CC configurable vibrations from the graphene, peaks at 1453 and 1389 cm−1 exhibited the stretching vibration and deformation vibration of hydroxy group. Moreover, an additional peak at 591 and 542 cm−1 in Fig. 2b could be ascribed to lattice absorption of Fe–O, further confirming the existence of SrFe12O19.19
As shown in Fig. 3a, a sharp peak at 2θ = 10.6° can be indexed to the (001) crystallographic plane of the GO. However, it vanished and a new characteristic (002) diffraction peak appeared at 2θ = 25.1° after the hydrothermal reduction (Fig. 3b). It was noteworthy that the broadening and weakening of the (002) diffraction peak of graphene was obvious, indicating the reduction process cannot restore graphene to the highly ordered crystal structure of graphite. The SrFe12O19 and SrFe12O19/G composites exhibited the very similar diffraction peaks, as shown in Fig. 3c and d. And the Rietveld refinement of XRD patterns of SrFe12O19/G composites was shown in Fig. S1.† The (001) crystallographic plane of the GO disappeared in the XRD pattern of SrFe12O19/G composites, suggesting the reduction of GO after the hydrothermal reaction.3 Nevertheless, no (002) diffraction peak of graphene appeared, which may be caused by two reasons. First of all, the in situ growth of SrFe12O19 nanoparticles on the graphene inhibited the re-stacking of graphene layers during the reduction process, weakening its diffraction intensity. Moreover, the diffraction peak of graphene was easy to be suppressed by SrFe12O19 due to the loading content of graphene in the composites.23,24 All labeled diffraction peaks in the range of 5–70° can be indexed to the hexagonal SrFe12O19 (PDF card no. 33-1340) crystallites.25,26 The sharp diffraction peaks and high intensity indicated the good crystallinity of as-obtained composites.
XPS was also employed to analyze GO and the SrFe12O19/G composites. The wide scan XPS spectrum (Fig. 4a) of the SrFe12O19/G composites showed photoelectron lines at a binding energy of 133.1, 284.6, 530.2 and 710.9 eV attributed to Sr 3d, C 1s, O 1s and Fe 2p, respectively. The inset in Fig. 4b showed the C 1s of GO, which consisted of two main components arising from C–C/CC (284.6 eV) and C–O (286.6 eV) groups and two minor components from CO (288.2 eV) and O–CO (289.4 eV) groups.3,17 Compared with GO, the C 1s of SrFe12O19/G composites varied dramatically. The content of C–O group decreased rapidly, and peaks of CO and O–CO groups even disappeared, suggesting a remarkable reduction after the hydrothermal reaction. In Fig. 4c, the Sr 3d5/2 signal appeared at 133.3 eV, and the peak at 134.9 eV was ascribed to the Sr 3d3/2 level. Fig. 4d showed the spectrum of Fe 2p region. The peaks of Fe 2p3/2 and Fe 2p1/2 were located at 711.6 and 724.8 eV, respectively. All the above analysis indicated the successful synthesis of the SrFe12O19/G composites.
Fig. 4 XPS spectra of the (a) survey scan, (b) C 1s region (the inset shows C 1s of GO), (c) Sr 3d region, (d) Fe 2p region of the SrFe12O19/G composites. |
Magnetic hysteresis loops of the SrFe12O19/G composites and SrFe12O19 particles were shown in Fig. 5. The saturation magnetization and coercivity of the SrFe12O19 particles were 61.2 emu g−1 and 2312.2 Oe, respectively. It can be observed that the saturation magnetization dropped dramatically with the introduction of nonmagnetic graphene. For the SrFe12O19/G composites, the saturation magnetization and coercivity were 41.6 emu g−1 and 1695.6 Oe, respectively.
A vector network analyzer was used to measure the electromagnetic parameters of the as-prepared SrFe12O19/G composites in the frequency range of 1–18 GHz. The complex permittivity and complex permeability of the SrFe12O19/G composites and the SrFe12O19 particles are shown in Fig. 6 and 7, respectively. As we know, the real part of complex permittivity (ε′) and complex permeability (μ′) stand for the storage ability of electromagnetic energy, and the imaginary part of complex permittivity (ε′′) and complex permeability (μ′′) represent the electromagnetic energy loss ability.27 For the SrFe12O19/G composites, the ε′ showed an approximately constant around 3.9 in the range of 1–18 GHz, while the ε′′ exhibited four high fluctuations from 0.5 to 2.7 in the whole frequency range. According to free electron theory,28 ε′′ ≈ 1/2πε0ρf, where ρ is the resistivity. It can be speculated that the lower ε′′ values represent higher electric resistivity. In general, the high electric resistivity is in favor of building a balance between complex permeability and complex permittivity, thus decreasing the reflection coefficient of the absorbing materials. Meanwhile, the μ′ and μ′′ changed gently in the range of 1–18 GHz. μ′ and μ′′ maintained at around 1.0 and 0.1, respectively. The dielectric loss tangent indicates the inherent dissipation of electromagnetic energy for dielectric materials. It can be seen from Fig. 6c that the dielectric loss tangent showed a similar variation tendency with ε′′. Four sharp peaks appeared at 4.4, 9.9, 15.1 and 17.5 GHz, and the peak values were 0.29, 0.54, 0.73 and 0.71, respectively. Meanwhile, the magnetic loss tangent increased from 0.08 to 0.13 at the 1.0–7.1 GHz range, and decreased from 0.13 to 0.08 over 7.1–18.0 GHz. Apart from dielectric loss and magnetic loss, another significant factor affecting electromagnetic wave absorption is impedance match characteristic, too high permittivity of absorber is detrimental to the impedance match and results in strong reflection and weak absorption.
Fig. 6 The complex permittivity (a), complex permeability (b), dielectric loss tangent (c), magnetic loss tangent (d) of the SrFe12O19/G composites. |
Fig. 7 The complex permittivity (a), complex permeability (b), dielectric loss tangent (c), magnetic loss tangent (d) of the SrFe12O19 particles. |
The complex permittivity, complex permeability, dielectric loss tangent and magnetic loss tangent of the SrFe12O19 particles are shown in Fig. 7a–d, respectively. Both the ε′ and ε′′ showed a downward trend in the range of 1–18 GHz, declining from 4.4 and 2.0 to 1.6 and 0.6, respectively. The μ′ kept unchanged around 2.0 in the range of 1.0–13.2 GHz, and then went up to 2.3 over 13.2–18.0 GHz. The μ′′ remained constant at about 0.08 in the whole frequency range. Compared with the SrFe12O19/G composites, the SrFe12O19 particles exhibited much lower dielectric loss tangent (less than 0.5) and magnetic loss tangent (around 0.025). Thus, it would be safe to conclude that the SrFe12O19/G composites exhibited better electromagnetic properties than the SrFe12O19 particles.
The RL can be calculated from the complex permeability and complex permittivity at the given absorber thickness and frequency using the following equations:
(1) |
While the normalized input impedance (Zin) is calculated by:
(2) |
εr = ε′ − jε′′, μr = μ′ − jμ′′ | (3) |
The RL curves of the SrFe12O19 particles and the SrFe12O19/G composites with different thicknesses are shown in Fig. 8. The RL is expected to be as low as possible at a given sample thickness. The minimum RL of the SrFe12O19 particles at the thickness of 4 mm reached −13.5 dB, and the effective absorption frequency (RL < −10 dB) ranged from 12.9 to 17.5 GHz. However, for the SrFe12O19/G composites, the minimum RL of −34.8 dB was observed at 13.6 GHz with a thickness of 3 mm, and the effective absorption frequency ranged from 11.7 to 17.4 GHz. All these analysis suggested that the SrFe12O19/G composites exhibited much better microwave absorbing properties than the SrFe12O19 particles.
Fig. 8 The calculated reflection loss of (a) the SrFe12O19 particles, (b) the SrFe12O19/G composites with different thicknesses. |
The related literatures based on SrFe12O19 were listed in Table 1. Wang et al.29 synthesized SrFe12O19–MWCNTs composites with different MWCNTs content by sol–gel method. The results indicated that 6 wt% SrFe12O19–MWCNTs composites possessed the best magnetic and wave absorbing properties. Poorbafrani et al.30 firstly prepared SrFe12O19 by sol–gel method, then combined with different concentrations of ZnO and obtained SrFe12O19/ZnO composites. They found the reflection loss (RL) in the Ku frequency band (12–18 GHz) was enhanced by up to 5 dB for 15% of ZnO in the nanocomposites. Chen et al.31 synthesized SrFe12O19/ZnFe2O4 composites with different weight ratios of SrFe12O19 to ZnFe2O4 using sol–gel technique. The composite powder with 15 wt% ZnFe2O4 possessed good microwave absorption properties. The minimum RL of the composite powder reached −37 dB at the thickness of 2.2 mm. He et al.32 synthesized a new type of conductive and magnetic PANI/Ag/SrFe12O19 composites via three-step method. The RL of the composites was below −10 dB between 8.7 GHz and 12.1 GHz, with a minimum loss value of −14.86 at 9.98 GHz. Chen et al.33 prepared lanthanum substituted strontium ferrite Sr1−xLaxFe12O19 (x = 0.05, 0.1, 0.15, 0.2) by a sol–gel process. The results showed that the minimum RL of the Sr1−xLaxFe12O19 (x = 0.15) reached −41.7 dB with the −10 dB bandwidth over 4 GHz at the thickness of 2.3 mm.
Samples | Parameters | ||
---|---|---|---|
Minimum RL (dB) | Frequency (GHz) | Effective bandwidth (GHz) | |
SrFe12O19–MWCNTs | −19.7 | 3.2 | Not mentioned |
SrFe12O19/ZnO | −15.47 | 8.37 | Not mentioned |
SrFe12O19/ZnFe2O4 | −37 | 8.7 | 3.9 |
PANI/Ag/SrFe12O19 | −14.86 | 9.98 | 3.4 |
Sr1−xLaxFe12O19 | −41.7 | 9.0 | 4 |
This work | −34.8 | 13.6 | 5.7 |
The enhanced absorbing properties of as-obtained composites can be attributed to three reasons. First of all, the conductive graphene with two dimensional planar structures constructed an effective conductive network in the composites, providing high dielectric loss tangent.17 Moreover, the well dispersion of homogenous SrFe12O19 nanoparticles on the graphene support ensured the pronounced absorbing performances. In addition, interface scattering could be generated owing to the difference in complex permittivity between graphene and SrFe12O19 nanoparticles, leading to more efficient absorption of electromagnetic waves. The absorbing mechanism diagram of SrFe12O19/G composites was illustrated in Fig. 9.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/c7ra05700h |