aSchool of Materials Science and Engineering, Shanghai University, Shanghai 200444, China. E-mail: junluo@shu.edu.cn
bThin Film Optoelectronic Technology Center, Shanghai Advanced Research Institute, Chinese Academy of Sciences, Shanghai 201210, China. E-mail: chenhy@sari.ac.cn; Tel: +86 21 20350846
First published on 23rd August 2017
Cu-doped p-type Bi0.5Sb1.5Te3 compounds have been prepared by a facile hydrothermal method. X-ray powder diffraction analysis shows that the lattice parameter decreases with the Cu content, indicating that Cu+ ions are distributed on the crystal site of Bi/Sb, which is further confirmed by the p-type conducting behavior of the Cu-doped Bi0.5Sb1.5Te3. With the addition of Cu, the hole carrier concentration increases, and meanwhile the lattice thermal conductivity decreases. Furthermore, the greatly raised hole carrier concentration effectively suppresses the bipolar effect, which is beneficial for improving the thermoelectric properties. A dimensionless thermoelectric figure of merit (ZT) value of ∼1.2 at room temperature is achieved for the sample with 0.6 wt% Cu (nominal composition), and the ZT value increases with the temperature to ∼1.5 at 150 °C. Cu-doped Bi0.5Sb1.5Te3 samples exhibit most excellent thermoelectric performance among the presently available (Bi,Sb)2Te3-based materials, implying great potential as near room temperature thermoelectric materials.
ZT = Sσ2T/κ, | (1) |
Bi2Te3-based materials3–9 are classical room-temperature thermoelectric materials. Both p-type (BixSb1−x)2Te3 (ref. 10 and 11) and n-type Bi2Se3−yTey (ref. 6 and 12–14) present excellent thermoelectric performance and have been put into commercial applications, which are well known as the most efficient thermoelectric materials operating near room temperature.15,16 According to literature reports, the Bi0.5Sb1.5Te3 alloy possesses the highest ZT value in all Bi2−xSbxTe3 solid solutions.17,18 Many methods have been attempted to fabricate Bi2Te3-based materials, e.g. ball milling,19–21 sintering22,23 and hot deformation.24–27 However, sample preparation needs a long time by most of the synthesis methods.17,28–31 Instead, hydrothermal synthesis as an effective method to fabricate Bi2Te3-based materials takes much shorter time,32,33 while the synthesis of a single-phase Bi0.5Sb1.5Te3 solid solution by hydrothermal reaction is rarely reported.18,34,35 Furthermore, the reported room-temperature thermoelectric properties of the Bi2Te3-based alloy synthesized by the hydrothermal method are not as good as expected.18,35,37 Therefore, it is desirable to develop a facile hydrothermal method to prepare an ideal single-phase Bi0.5Sb1.5Te3 alloy with optimized thermoelectric properties.
In this work, Cu-doped Bi0.5Sb1.5Te3 samples have been prepared by a facile hydrothermal method. According to the result of structure analysis, single-phase alloys with excellent thermoelectric properties have been successfully synthesized. A room-temperature ZT value as high as ∼1.2 has been achieved for the sample doped with nominal 0.6 wt% Cu, and its maximum ZT value of ∼1.5 is obtained at 423 K. To our knowledge, the nominal 0.6 wt% Cu-doped Bi0.5Sb1.5Te3 sample synthesized by a hydrothermal method in our experiments exhibits the most excellent thermoelectric performance among the presently available (Bi,Sb)2Te3-based materials, showing the great potential as near room temperature thermoelectric material.
X-ray powder diffraction (XRD) patterns were collected on a Bruker AXS D8 Advance Diffractometer with Cu Kα radiation (λ = 0.154056 nm) using the continuous scanning method with a scanning voltage of 40 kV and a scanning speed of 0.01° per step. The morphologies of the samples were observed on a Hitachi S-4800 scanning electron microscope (SEM). LSR-3/1100 thermoelectric measurement system was used to measure the Seebeck coefficient and resistivity. The thermal diffusivity of the sample was detected by a laser flash diffusivity method on a Netzsch Laser Flash Apparatus (LFA) 1000. The total thermal conductivity κ was calculated by the equation κ = DρCp, where D, ρ and Cp were the thermal diffusivity, the mass density and the volumetric specific capacity of the sample, respectively. Cp was measured by a Netzsch differential scanning calorimetry (DSC) 201F1 instrument, and ρ by the Archimedes-method.
Fig. 1 XRD patterns of the samples S1–S4. (Nominal Cu contents of S1, S2, S3 and S4 are 0 wt%, 0.6 wt%, 1.6 wt% and 2.6 wt%, respectively). |
Samples | Nominal Cu content x (wt%) | a (Å) | c (Å) | V (Å3) |
---|---|---|---|---|
S1 | 0 | 4.3094 (±0.0016) | 30.487 (±0.0007) | 490.31 (±0.0020) |
S2 | 0.6 | 4.3015 (±0.0011) | 30.473 (±0.0006) | 488.31 (±0.0015) |
S3 | 1.6 | 4.2986 (±0.0018) | 30.466 (±0.0009) | 487.53 (±0.0025) |
S4 | 2.6 | 4.2914 (±0.0024) | 30.473 (±0.0011) | 486.00 (±0.0030) |
Fig. 2 Room-temperature hole carrier concentration as a function of the nominal Cu content for all Bi0.5Sb1.5Te3 samples. |
To further explore the structural feature of Cu-doped Bi0.5Sb1.5Te3, the morphologies of the as-prepared powder and hot-pressed bulk sample have been observed by SEM. Fig. 3a and b show the SEM images of sample S3, exhibiting the feature of small particle sizes. As shown in Fig. 3a, most of the particles are at the nanoscale, typically on the order of several hundreds of nanometers. Furthermore, some mesoscale hexagonal platelets with the particle sizes from 1 to 10 micrometers are observed in Fig. 3a, which should relate to the anisotropic crystal structure of Bi0.5Sb1.5Te3. The Bi2Te3 compound has a rhombohedra structure32 with the space group Rm, wherein along the c-axis, the atomic layers array in the order of –Te(1)–Bi–Te(2)–Bi–Te(1)– and the neighboring Te(1) layers are linked by weak van der Waals bonds.34–37 Therefore, the morphology of Bi2Te3-based alloy normally exhibits the feature of hexagonal platelets. For the powders obtained in our work, under the control of hydrothermal synthesis, most of grains are nanoparticles with deficient crystallinity, while only a small number of grains are well-crystallized, existing as hexagonal platelets. This could also explain the isotropic properties of these samples (see Fig. S1 and S2†). As shown in Fig. 3b, the small particle size is maintained after hot pressing (the feature of small particle size can also be observed from the cross section of the bulk, shown in Fig. S3†). Hence, the small particle size as well as numerous grain boundaries of the samples synthesized by the hydrothermal method could contribute to the reduced lattice thermal conductivity around room temperature, which is beneficial for the Cu-doped Bi0.5Sb1.5Te3 aiming at room-temperature applications.
Fig. 3 Typical SEM images of (a) the as-prepared powders and (b) ground powders after the hot pressing of sample S3. |
Fig. 4 shows the electrical transport properties of the undoped and Cu-doped Bi0.5Sb1.5Te3 samples. As shown in Fig. 4a, the Seebeck coefficients of all the samples are positive, further confirming their p-type conducting behavior. The room-temperature Seebeck coefficient decreases with the Cu content because of the increased carrier concentration. For the undoped sample S1, its Seebeck coefficient decreases with the increasing temperature, which can be ascribed to the bipolar effect caused by the intrinsic excitation below room temperature.30,35 For the Cu-doped samples S2–S4, their room temperature Seebeck coefficients decrease with the increase of Cu content, which can be attributed to increased hole concentration by substituting of Cu for Bi/Sb. Furthermore, their temperature-dependent Seebeck coefficients show the typical behavior of a degenerate semiconductor. As shown in Fig. 4a, for samples S2–S4, the Seebeck coefficient firstly increases linearly with the increasing temperature, but linear trend of the Seebeck curve is suppressed by the bipolar effect at elevated temperature. It is obvious that the bipolar effect of the Cu-doped samples shifts to higher temperature because the mixed conduction is suppressed by increasing hole concentration. Thus, comparing with the undoped sample, the Seebeck coefficients of the Cu doped samples increase dramatically in the temperature range of 150–350 °C.
Fig. 4 Temperature-dependences of (a) Seebeck coefficient and (b) electrical conductivity of undoped and Cu-doped samples. |
As shown in Fig. 4b, the temperature-dependent electrical conductivity of the undoped sample S1 also shows the conducting behavior of intrinsic excitation, i.e. the electrical conductivity increases with the increasing temperature. For the Cu-doped samples, their electrical conductivities firstly decrease rapidly with the raised temperature, and then decrease slowly with the temperature due to the mixed conduction. The slowly decrease of electrical conductivity at high temperature for all the samples can be ascribed to the bipolar effect. Furthermore, the doping of Cu increases the hole concentration, which effectively suppresses the bipolar effect and shifts the intrinsic excitation temperature to higher temperature. It is worth to note that the σ values of the Cu-doped samples prepared via a facile hydrothermal method in our work could be comparable to that of Bi–Sb–Te alloys synthesized by conventional sintering methods,30,39 indicating this facile hydrothermal method is an effective route for developing high-performance (Bi,Sb)2Te3-based materials.
It should be pointed out that the room-temperature electrical conductivity is almost the same for the samples S2 and S3. To clarify this, Hall carrier concentration and mobility have been measured. As listed in Table 2, the hole concentration of sample S3 is almost twice of that of the sample S2, while its mobility is nearly half of that of the latter one. Hence, these two samples have similar electrical conductivity at room temperature. The reduced carrier mobility of the sample S3 could be ascribed to the enhanced carrier scattering in two aspects: (1) more lattice point defects produced by Cu substitution and (2) increased hole concentration.
Samples | Nominal Cu content x (wt%) | n (1019/cm3) | μ (cm2 V−1 s−1) |
---|---|---|---|
S2 | 0.6 | 6.7792 | 60.7478 |
S3 | 1.6 | 13.9000 | 29.2516 |
The combination of raised Seebeck coefficient and increased electrical conductivity results in a power factor of ∼25 μW cm−1 K−2 at 50 °C for sample S2 (Fig. 5), which is nearly 9 times as large as that of sample S1. The power factor decreases to 23 μW cm−1 K−2 at 150 °C and remains as high as ∼8.5 μW cm−1 K−2 at 350 °C for sample S2. Furthermore, the power factors of Cu-doped samples are always much larger than that of undoped sample in the measured temperature range from 50 °C to 350 °C.
Fig. 6 shows the temperature-dependent thermal conductivity of samples S1–S4. It is obvious that all the samples have very low thermal conductivities. As shown in Fig. 6, the thermal conductivity of sample S1 increases with the increasing temperature, which could be ascribed to the increased electronic contribution to the total thermal conductivity caused by the bipolar effect. Similarly, for the Cu-doped samples, the increase of the thermal conductivity at high temperature can also be attributed to intrinsic excitation.
The thermal conductivity of Cu-doped samples S2–S4 is higher than that of the undoped sample S1 owing to the dramatically increased electronic thermal conductivity, since the hole concentration is significantly enhanced with the Cu content.
For undoped sample S1, compared with those synthesized by mechanical alloying19 and spark plasma sintering (SPS),39 its nanostructuring obtained by hydrothermal synthesis lowers the thermal conductivity by about 31–50% at room temperature, due to the contribution of additional phonon scattering, implying that our hydrothermal synthesis method is effective on reducing the thermal conductivity. As for sample S2, its average thermal conductivity in the temperature range of 150–350 °C is about 0.71 W m−1 K−1, approximately 12%, 21% and 22% reduction than those of Cu-doped Bi–Sb–Te samples reported by Lee et al.,17 Hao et al.38 and Cui et al.,30 respectively. The low thermal conductivity of sample S2 can be ascribed to different defects: nanoscale grains by hydrothermal synthesis, atomic-scale point defects of Cu substitution for Bi3+/Sb3+, and the presence of second phase. It is worth to note that, in p-type Bi0.5Sb1.5Te3 materials, the Cu dopants not only increase the hole concentration, but also introduce nanostructural defects, which were also observed in SPS-treated Cu-doped Bi0.5Sb1.5Te3 bulk samples.38
Fig. 7 presents the ZT values for the undoped and Cu-doped samples. The ZT value of sample S1 decreases with the increasing temperature, which can be explained by a drastic reduction of the Seebeck coefficient due to the bipolar effect. The doping of Cu effectively suppresses the bipolar effect by increasing the hole concentration, leading to a shift of the peak ZT value to higher temperature with the raised Cu concentration. Obviously, the ZT values of the samples with Cu doping are much larger than those of the undoped sample, even though the total thermal conductivity is enhanced after the Cu doping. Therefore, the huge enhancement of ZT from 50 °C to 350 °C is mainly contributed from the power factor afforded by doping. However, with the further increased Cu content, the ZT value decreases, which probably originates from the increased electronic contribution to the thermal conductivity due to the increasing electrical conductivity. The sample with nominal 0.6 wt% Cu exhibits the best thermoelectric performance because of the appropriate doping level, small grain size, as well as the presence of trace amount of impurities. Finally, a ZT value of 1.2 around room temperature and a peak ZT value of ∼1.5 at 150 °C are achieved for the sample S2. The average ZT value of sample S2 in the temperature range of 50–200 °C is about 1.4, ∼40% improvement of that of the commercial Bi2Te3 ingot materials. It should be noted that, by the Cu doping, the optimum operating temperature is decreased and the working temperature range becomes broader, making Cu-doped bismuth antimony telluride based alloys have better prospects for commercial applications.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/c7ra06277j |