Dan Xiaa,
Yongchao Luoa,
Qiang Li*b,
Qingzhong Xuec,
Xiaomin Zhanga,
Chunyong Liang*a and
Mingdong Dong*d
aResearch Institute for Energy Equipment Materials, Collage of Materials Science and Engineering, Tianjin Key Laboratory of Materials Laminating Fabrication and Interface Control Technology, Hebei University of Technology, Tianjin 300130, China. E-mail: liangchunyong@hebut.edu.cn
bKey Laboratory for Colloid and Interface Chemistry, Ministry of Education, School of Chemistry and Chemical Engineering, Shandong University, Jinan 250100, Shandong, China. E-mail: qiang@sdu.edu.cn
cState Key Laboratory of Heavy Oil Processing, College of Science, China University of Petroleum, Qingdao 266580, Shandong, China
dInterdisciplinary Nanoscience Center (iNANO), Aarhus University, Aarhus C, DK-8000, Denmark. E-mail: dong@inano.au.dk
First published on 14th August 2017
The sliding behavior of interwalls between double-walled carbon nanotubes (DWCNTs) is studied by molecular dynamics (MD) simulations. The results show that a platinum (Pt) nanowire (NW) is able to push out a single wall from the DWCNT. The pushout process is strongly dependent on the match level of the NW radius and the inner wall CNT radius. The match radius of the Pt NW and the inner CNT wall will form perfect single-walled CNT (SWCNT) and Pt/CNT core/shell nanostructure. In addition, the bonding interactions between the Pt NW and the CNT are also studied. The shear stress between the Pt NW and CNT is in megapascal magnitude. The chirality has little effect on the interfacial bonding and the shear stress between the Pt NW and the CNT. This study will shed light on the understanding of the lubrication mechanism of the multi-walled CNT and the metal NWs in realistic situations.
To utilize MWCNTs in micro/nanomechanical systems, achieving a comprehensive understanding of their nanomechanical and nanotribological properties is of significant importance. So far, plenty of studies have focused on the mechanical and nanotribological properties of MWCNTs. Kim and his colleagues successfully manipulated the MWCNTs by using atomic force microscopy.17 Ultralong MWCNTs were extracted shell-by-shell allowing the exposure of the innermost single-walled carbon nanotube (SWCNT), which changed the electrical characteristics of the MWCNTs. Wei and his colleagues pulled out the inner shells from centimeters-long double-walled carbon nanotubes (DWCNTs) by a steady gas flow under ambient condition,18 which show the superlubricity in centimeters-long DWCNTs. Because of the difficulty of nanomanipulation, more theoretical studies were performed regarding the sliding behavior between nested walls in MWCNTs than the direct experimental observation.9,19–21 Hu et al. studied the pullout process of some outer walls against other inner walls in MWCNTs and investigated the sliding behavior between nested walls.19 Curtin et al. studied the pullout forces and friction in MWCNTs.20 The key conclusion of these simulation studies showed that the pullout force was dominated by the end effect. Local pressure can generate local frictional sliding, and distributed pressure or defects in the nanotube walls can increase or decrease the pullout force, depending on the defect geometry, permitting stick-slip behavior as observed experimentally. In spite of these intriguing results, the extracted sliding behavior of the outmost wall in a MWCNT is still unclear. In particular, there is no general theory addressing the pushout behavior related to spontaneous sliding in a MWCNT by metal nanowires.
In this study, molecular dynamics (MD) simulations on the pushout process of the inner walls of various DWCNTs by platinum nanowires (Pt NWs) are carried out, aiming at understanding the inherit mechanism of the extracting sliding between nested walls and Pt NW. Because there is no chemical bond among DWCNT walls, the DWCNTs show structural superlubricity.22 When the interaction energy between the outmost wall and the Pt NW is larger than that between nested walls, the Pt NW is able to push out the inner wall in DWCNTs. The results show that the diameter of the inner wall of DWCNTs affects the pushout process significantly. However, the chirality of both the inner and outer wall has little effect on the extraction. In addition, the Pt NW with match diameter can also successfully extract the outmost wall in a corresponding MWCNT. The Pt NW length has little effect on the extraction sliding. The study here will help us understanding the inherit mechanism of the extracting sliding, which is essential for nano-mechanical engineering system. Since the successful pushout will result in a SWCNT and a Pt NW/CNT core/shell nanostructure for a DWCNT. This may provide potential applications in many new areas, for example, artificial muscle application.23
Etotal = Evalence + Ecross-term + Enon-bond | (1) |
The valence energy, Evalence, is generally accounted for diagonal terms, including bond stretching, valence angle bending, dihedral angle torsion, inversion, also called out-of-plane interactions (oop) terms and a Urey–Bradley (UB) term.
Evalence = Ebond + Eangle + Etorsion + Eoop + EUB | (2) |
The cross-term interaction energy, Ecross-term, accounts for factors such as bond or angle distortions caused by nearby atoms to accurately reproduce experimental vibrational frequencies and the dynamic properties of molecules. Cross terms can include the following: stretch–stretch, stretch–bend–stretch, bend–bend, torsion–stretch, torsion–bend–bend, bend–torsion–bend and stretch–torsion–stretch.
Ecross-term = Ebond–bond + Eangle–angle + Ebond–angle + Eend-bond–torsion + Emiddle-bond–torsion + Eangle–torsion + Eangle–angle–torsion | (3) |
The non-bond interaction term, Enon-bond, accounts for the interactions between non bonded atoms, including vdW, electrostatic and hydrogen bond.
Enon-bond = EvdW + ECoulomb + EH-bond | (4) |
The equation of Evalence, Ecross-term and Enon-bond are listed as following:
(5) |
(6) |
(7) |
The main modeling system is composed of a DWCNT and a Pt NW (Fig. 1a). Periodic boundary conditions are applied in the x and y-directions of the modeling system. The length of all the DWCNTs is around 50 Å while the diameter is various. The unsaturated boundary effect is avoided by adding hydrogen atoms at both ends of the DWCNTs. The Pt NW was constructed by the atom selection of the Pt supercell. The Pt unit cell with the face-centered cubic structure parameter (a = b = c = 3.924 Å; α = β = γ = 90°) was imposed from the Materials Studio software. The length of the Pt NW is 54.9 Å while the radius is various.
Fig. 1 Snapshots of the pushout process. A Pt NW (r = 5 Å) pushes out the inner wall of a DWCNT at (a) 0, (b) 5, (c) 45, (d) 90, (e) 225 and (f) 450 ps, respectively. |
In the simulations, all the models are subjected to a canonical (NVT) ensemble, carried out at a temperature of 300 K and an integration time step of 1 fs. Temperature control is achieved using an Andersen feedback thermostat. The energy of the system is minimized to achieve the strongest bonding between the CNT and Pt NW. To elucidate the results of the MD simulations, the interaction energy, the interaction bonding energy and interfacial shear stress between the CNT and NW are calculated and discussed accordingly.
ΔE = Ecom − (ECNT + ENW) | (8) |
(9) |
The process of pushing out is achieved by pushing out the inner wall using a Pt NW. The pushout energy (Epushout) is defined as the energy difference between the fully embedded nanotube and the completed pushout configuration.
Epushout = E1 − E0 = (ΔE1 + ECNT1 + ENW1) − (ΔE0 + ECNT0 + ENW0) = (ΔE1 − ΔE0) + (ECNT1 − ECNT0) + (ENW1 − ENW0) | (10) |
The pushout energy can be divided into three terms, where E1 and E0 are the potential energy of the composite after and before the pushout process, respectively. ECNT and ENW are the potential energy of the CNT and the Pt NW, respectively. ΔE is the interaction energy between the DWCNT and Pt NW. The pushout energy can be related to the interfacial shear stress, τi, by the following relation:
(11) |
(12) |
The energy plots during the pushout process are shown in Fig. 2a–c. Before t = 45 ps, the interaction energy increases slightly, because of the domination of the interaction between the inner wall and the Pt NW, inducing the attraction of the inner wall towards the Pt NW. However, the pushout energy decreases dramatically from 1000 kcal mol−1 to 139 kcal mol−1. The interfacial bonding energy drops from −14 kcal mol−1 Å2 to −0.36 kcal mol−1 Å2. After t = 45 ps, the interaction energy between the DWCNT and Pt NW starts to increase dramatically, due to pushing the inner wall back to outer wall. Meanwhile, the pushout energy continues to decrease with a smaller decreasing slope and the interfacial bonding energy starts to increase slightly. At t = 90 ps, the Pt NW pushes the inner wall back to the outer wall. The pushout energy starts to change from positive value to negative value while the interaction energy and the interfacial bonding energy continue to increase. Afterwards, the Pt NW continues to push the inner wall along the axial direction. The interaction energy, the pushout energy and the interfacial bonding energy are all increased. The only difference is the interfacial bonding energy reaches the equilibrium at a shorter time (around t = 300 ps) compared to that of the interaction energy and the interfacial bonding energy (around t = 450 ps).
The center of mass (COM) distances between each CNT and Pt NW and between nested walls in DWCNT are shown in Fig. 1d. It clearly shows that the COM distance between the inner wall and Pt NW decreases in the beginning because of the reform of the Pt NW. At t = 45 ps, the inner wall and the Pt NW reaches the optimum state and keep this optimum distance till the completion of the remaining pushout process. The initial negative value and the later positive value of the COM distance between the inner wall and the outer wall indicates the opposite movement direction of both CNTs. The COM distance between the outer wall and the Pt NW decreases along the whole pushout process and reaches the equilibrium at t = 450 ps. The radius distribution functions of the whole system before and after the pushout process are shown in Fig. 1e and f. Before the pushout process, the Pt NW is well organized. The projected radius distance between the outer shell and the Pt NW is ∼3.2 Å while the projected radius distance between the nested walls is ∼3.8 Å, which is a bit larger than the ideal value of 3.4 Å.30,31 In addition, the projected radius distance between the inner wall and the second row of Pt particle in Pt NW is 2.6 Å, and the projected diameter of the inner wall is 7.8 Å, which is smaller than the ideal value of 8.1 Å. After the completing of the pushout process, the re-organized Pt NW inserted into the outer wall inducing pushing out of the inner wall. The projected radius distance between the outer wall and the Pt NW is almost the same as before the pushout process, and so does the projected radius distance between the inner wall and the second row of Pt particle in Pt NW. As the inner wall has been pushed out from the outer shell, these two SWCNTs are no longer packed parallel, thus the two peaks disappeared. All the small peaks along the line plot (Fig. 1f) indicate the badly organized of the model along the project radius direction.
Energy components (kcal mol−1) | Status I (t = 0 ps) | Status II (t = 500 ps) |
---|---|---|
Valance energy | 67096.361 | 68377.499 |
Bond | 346.380 | 832.964 |
Angle | 63.360 | 459.561 |
Torsion | 66337.960 | 66605.121 |
Inversion | 348.661 | 479.853 |
Cross terms | −1023.139 | −828.036 |
stretch–stretch | 74.445 | 16.228 |
stretch–bend–stretch | −51.327 | −46.173 |
stretch–torsion–stretch | −1578.263 | −1145.741 |
Separated–stretch–stretch | 123.131 | 56.971 |
Torsion–stretch | 200.623 | 130.171 |
Bend–bend | 0.000 | 0.000 |
Torsion–bend–bend | −0.892 | −0.056 |
Bend–torsion–bend | 209.143 | 160.565 |
Non-bond energy | 605.842 | −18204.903 |
van der Waals | 561.520 | −18228.571 |
Long range correction | −4.578 | −6.177 |
Electrostatic | 48.901 | 29.846 |
Total energy | 66679.064 | 49344.561 |
The schematic mechanism of the pushout process is shown in Fig. 3. For an ideal DWCNT with partly extruded inner wall by Pt NW, the vdW interaction between the DWCNT and the Pt NW can be divided into three sections (Fig. 3a). Section I indicates the overlapped region between adjacent walls (including the vdW interaction length region where the inner wall is not covered by the outer wall); section II indicates the overlapped region between outer wall and Pt NW (including the vdW interaction length region where the Pt NW is not covered by the outer wall); section III indicates the interface between the inner wall and Pt NW covered by the outer wall. In sections I and II, the axial component of vdW force is nearly zero as a direct consequence of the counteraction of multiple vdW interactions during the pushout process. The pushout force which equals the total shear force induced by the shear stress τi on the sliding surface is in equilibrium with the axial component of vdW force. Therefore, the pushout force is nearly zero which induces zero pushout energy (sections I and II). Since the whole process is dynamic, section I region will decrease while section II region will increase during the pushout process. Considering the cut-off distance of the vdW interaction of 0.95 nm, it will repetitive breaking and reforming of vdW interaction between adjacent walls and between outer wall and Pt NW during the dynamic pushout process. Mainly the axial component of vdW force difference (FvdW2 − FvdW1) in section III contributes to the pushout force completing the pushout process. When the vdW force between the outer wall and the Pt NW, FvdW2, is larger than that between the nested walls, FvdW1, the Pt NW can push out the inner wall due to the low friction between nested walls in the DWCNTs. The vdW energy evolution during the pushout process is shown in Fig. 3b. It shows that the vdW energy changes from positive value to negative value due to the vdW interaction changing from the DWCNT dominant to DWCNT outer wall-Pt NW dominant.
DWCNTs | Diameter of inner CNT Di (Å) | Diameter of outer CNT Do (Å) | Diameter difference ΔD (Å) |
---|---|---|---|
DWCNT (6, 6)/(16, 6) | 8.14 | 15.42 | 7.28 |
DWCNT (7, 7)/(17, 7) | 9.49 | 16.74 | 7.25 |
DWCNT (8, 8)/(18, 8) | 10.85 | 18.06 | 7.21 |
DWCNT (9, 9)/(19, 9) | 12.20 | 19.38 | 7.18 |
DWCNT (10, 10)/(20, 10) | 13.56 | 20.71 | 7.15 |
DWCNT (11, 11)/(21, 11) | 14.92 | 22.05 | 7.13 |
DWCNT (12, 12)/(22, 12) | 16.27 | 23.38 | 7.11 |
Meanwhile, the energy plots of the interaction between the Pt NW and different diameter of sequence DWCNTs are shown in Fig. 4b–d. Since DWCNT (10, 10)/(20, 10) and DWCNT (11, 11)/(21, 11) are not able to complete the pushout process, the energy plots are not shown. The interaction energies between diverse DWCNTs and Pt NWs are shown in Fig. 4b. During all the pushout process, the interaction energy increases in the beginning and then decrease gradually. When the pushout process changed to the inserting process, the interaction energy starts to increase. The interfacial bonding energy (Fig. 4c) decreases linearly with increasing the diameter of the DWCNTs. The shear stress (Fig. 4d) shows the same tendency as the interaction energy, which increases in the beginning and then decreases with increasing diameters of DWCNTs, finally increase when the diameter of inner wall is larger enough than that of Pt NW.
The COM distances between the inner and outer walls are shown in Fig. 4e. The negative value indicates the pullout process while the positive value indicates the pushout process. The platform indicates the steady status of the system. It is obvious that some of the pushout process experience the medium steady state before the completion of the pushout process (the final platform). The smaller COM values of the DWCNT (7, 7)/(17, 7), DWCNT (8, 8)/(18, 8) and DWCNT (9, 9)/(19, 9) than that of the DWCNT (6, 6)/(16, 6) indicate partly pushout of the inner walls. According to the COM distances between the nested walls, the average velocity of the pushout process are obtained (Fig. 4f). It apparently shows that the average velocity of the pushout process increases when the diameter of inner wall increases from 8.14 Å to 9.49 Å, which may be due to the less resistance with the increasing diameter. Further increase the diameter, the interaction between the nested walls become larger. Thus it become more and more difficult for Pt NW pushing out the inner walls completely. When the diameter of the inner wall is larger enough than the Pt NW diameter, the pushout process changes to the inserting process. In this consequences, all the resistance during the pushout process become the power benefit for the inserting process. Therefore, the average velocity increases dramatically.
DWCNTs | Inner wall chiral index (n, m) | Outer wall chiral index (n, m) | Di (Å) | Do (Å) | ΔD (Å) |
---|---|---|---|---|---|
1 | (7, 7) | (17, 7) | 9.49 | 16.74 | 7.25 |
2 | (8, 6) | (17, 7) | 9.52 | 16.74 | 7.22 |
3 | (9, 5) | (17, 7) | 9.62 | 16.74 | 7.12 |
4 | (10, 4) | (17, 7) | 9.78 | 16.74 | 6.96 |
5 | (11, 2) | (17, 7) | 9.49 | 16.74 | 7.25 |
6 | (12, 0) | (17, 7) | 9.39 | 16.74 | 7.35 |
7 | (7, 7) | (17, 6) | 9.49 | 16.18 | 6.69 |
8 | (7, 7) | (18, 6) | 9.49 | 16.94 | 7.45 |
9 | (7, 7) | (19, 3) | 9.49 | 16.18 | 6.69 |
10 | (7, 7) | (19, 4) | 9.49 | 16.66 | 7.17 |
11 | (7, 7) | (21, 1) | 9.49 | 16.85 | 7.36 |
To completely push the inner wall out of DWCNT outer shell, the length of the DWCNTs and Pt NWs are almost the same. The length of the Pt NW has little effect on the pushout process compared with the Pt NW diameter. Fig. 6b shows the inner wall of DWCNT (7, 7)/(17, 7) pushed out by the Pt NW with different lengths. It shows that the Pt NWs with different lengths are all able to push out the inner wall from the outer shell though the pushout length varies. Specifically the shorter Pt NW length, the shorter length of the inner wall was pushed out (Fig. 6b-iv). When the Pt NW length is longer than the DWCNT length, the inner wall is able to completely push out (Fig. 6b-vi).