Jiangyong Pan,
Jing Chen*,
Qianqian Huang,
Lixi Wang and
Wei Lei*
Joint International Research Laboratory of Information Display and Visualization, School of Electronic Science and Engineering, Southeast University, Nanjing, 210096, China. E-mail: chenjing@seu.edu.cn
First published on 7th September 2017
A high-performance solution processed quantum dot light emitting diode (QLED) has been fabricated via modulating the hole transport by doping 1-bis[4-[N,N-di(4-tolyl)amino]phenyl]-cyclohexane (TAPC) into poly-N-vinylcarbazole (PVK) as the hole transport layer (HTL). With a low doping content, the hole transport ability of the HTL can be enhanced due to the extremely high hole mobility of TAPC. However, increasing the doping ratio of TAPC excessively results in degraded performance of the QLED due to the deteriorated film quality and increased energy barrier from the HTL to the quantum dots (QDs), which is attributed to the relatively shallow position of the HOMO level for TAPC. Using the optimized composition ratio of the doped HTL (3:1 vol% of PVK:TAPC), the best QLED performance was achieved with a low turn-on voltage of 3.3 V due to the charge balance, which facilitates exciton recombination in the emissive layer (EML). In addition, the highest current efficiency (26.2 cd A−1), power efficiency (19.2 lm W−1), external quantum efficiency (6.2%) and 60% enhancement in the stability of the device were achieved. The improvement in the device performance can be attributed to the suppression of Auger recombination due to the balance of carrier injection into the emissive layer composed of QDs and the separation of the carrier accumulation zone from the exciton formation interface by the modulation of hole transport. The lowered turn-on voltage and improved efficiency presented here offer potential for high throughput and practical use for commercialized QLED displays.
A main obstacle towards improving QLED performance is intrinsic processes in the device, such as multicarrier Auger recombination or electron–hole separation due to applied electric field. Here we tried to solve the problem of Auger recombination, which impacts both QLED efficiency and the onset of efficiency roll-off at high currents.19 It has been found that the Auger recombination is attributed to charging of QDs with extra electrons due to the imbalance of charge transport.20 It is prone to the imbalance of charge in the conventional QLEDs due to the characteristic band structure of the component layers. The valence band (VB) (∼−6 eV to −7 eV) of QDs is usually much lower than the highest occupied molecular orbital (HOMO) of typical conjugated organic molecules or polymers, which are usually utilized as the hole transport layer (HTL), and the conduction band (CB) (∼−4 eV) is similar to that of metal oxide acting as the electron transport layer (ETL),21,22 thus the energy band of the QD is much more beneficial for electron injection than for hole injection, resulting in the imbalance of carrier transportation. Generally, the single layer of poly-N-vinylcarbazole (PVK) has been widely used as an HTL for QLEDs in the past two years.23 Compared with the other HTL materials, the HOMO level of PVK is rather low (∼−5.8 eV), but the hole mobility is quite small (2.5 × 10−6 cm2 V−1 s−1), which restricts the hole transport.24 Therefore, it is highly desirable to dope the HTL materials to modulate the hole transport in order to balance the carrier transport, leading to improvement in the QLEDs performance.
Recently, it has been attempted to adopt the hybrid HTL, which takes advantage of both deep HOMO level and high hole mobility of the components within the hybrid HTL. For instance, a proper blending ratio of poly-N-vinylcarbazole (PVK) and 4,4′,4′′-tris(N-carbazolyl)-triphenyl-amine (TCTA) has been utilized as the HTL in the QLEDs,25 as well as the blending of poly(4-butyl-phenyl-diphenyl-amine) (poly-TPD) and TCTA as the HTL reported by another group.26 However, the hole mobility of the blending material of TCTA is fairly low (2.0 × 10−5 cm2 V−1 s−1),27 which weakens the effect of band level adjustment and influences the hole transport. In addition, our group has tried to blend 4,4′-bis-(carbazole-9-yl)biphenyl (CBP) with PVK to function as the hybrid HTL. Although the performance of the optimized device was improved, it is still far away from the anticipated performance, which is primarily due to the poor film quality caused by the relatively low glass transition temperature (Tg of ∼62 °C) of CBP.28
Herein, we demonstrate highly improved performance of QLEDs by using PVK doped with 1-bis[4-[N,N-di(4-tolyl)amino]phenyl]-cyclohexane (TAPC), which has been used in the tandem OLED.29 The capability of hole transport in the blended HTL is modulated and enhanced by taking the advantages of high hole mobility of TAPC (1.0 × 10−2 cm2 V−1 s−1) in the OLED27 and superior energy level of PVK, leading to promoted balance of charge carrier injection and transport. The current efficiency, power efficiency and EQE increased to 26.2 cd A−1 and 19.2 lm W−1 and 6.2%, respectively. The mechanism of the improvement in the device performance will be discussed.
The characteristics of prepared ZnO have been studied further as displayed in Fig. 2. The ZnO NPs have the diameter of approximately 3.5 nm with the absorbance peak of 325 nm and PL peak of 545 nm. It can also be verified from the XRD pattern that our synthesized ZnO NPs have a wurtzite structure as shown in Fig. 2(c). In addition, the high electron mobility of ZnO has been measured to be 4 × 10−3 cm2 V−1 s−1 based on the TFT transfer characteristics of ZnO NP film as displayed in Fig. 2(d), which also makes ZnO a good candidate for the ETL. It is found that the holes are restricted due to the relatively low hole mobility of PVK and larger barriers (1.0 eV) at the interface of the HTL/EML compared with that of ETL/EML in the conventional QLED. The imbalance of carrier injection leads to the accumulation of excess electrons in the EML, which consequently enhances the non-radiative Auger assisted recombination or leak to the counter electrode without recombination, thus greatly reducing the efficiency and stability of the devices.20 Therefore, it is necessary to balance the electron and hole currents by promoting the hole transport. TAPC was introduced into PVK to form the doped HTL, taking its fairly high hole mobility into account.
Fig. 2 (a) The TEM image, (b) the absorption and PL spectra and (c) XRD image of ZnO NPs. (d) TFT transfer characteristics of ZnO nanoparticle film. |
For multilayer QLED devices, the surface roughness of underlayer have great effects on the uniformity of following deposited top layer, further influencing the device performance due to the usage of spin-coating technique.33 For this study, the QDs layer was spin-coated on the HTL layer, therefore the roughness of the HTL layer plays an important role in the film quality of the QDs deposition. As shown in Fig. 3 and Table 1, the bare PVK film coated on the PEDOT:PSS has the smallest roughness of root mean square (Rq) of 0.57 nm, while doping TAPC into PVK degrades the uniformity of the film due to the relatively low Tg of TAPC. In addition, it is worth noting that the uniformity of the film will deteriorate when the blend ratio of PVK exceeds 2:1.
Fig. 3 AFM image of different doped HTL coated on the PEDOT:PSS layer (a) PVK (b) PVK:TAPC = 5:1 (c) PVK:TAPC = 4:1 (d) PVK:TAPC = 3:1 (e) PVK:TAPC = 2:1 (f) PVK:TAPC = 1:1. |
The volume ratio of PVK and TAPC | ||||||
---|---|---|---|---|---|---|
PVK | 5:1 | 4:1 | 3:1 | 2:1 | 1:1 | |
Rpv (nm) | 4.33 | 5.57 | 5.84 | 6.37 | 7.42 | 10.9 |
Rq (nm) | 0.57 | 0.71 | 0.73 | 0.93 | 1.13 | 3.1 |
Ra (nm) | 0.45 | 0.56 | 0.58 | 0.78 | 1.01 | 2.25 |
The change of the energy band of the doped HTL should be evaluated seriously because of the difference of the energy band structure between these two HTL materials. Thus, the energy levels of doped HTL has been confirmed by the ultraviolet photoelectron spectroscopy (UPS) measurements. The resulting secondary-electron cutoff and valence-band regions are shown in Fig. 4(a) and (b), respectively. Generally, the work function (WF) could be estimated by the difference between the incident light energy (21.2 eV) and the energy of secondary cutoff.34 In this case, the PVK and PVK:TAPC films are calculated to be 4.75 eV and 4.65 eV, respectively, as labeled in Fig. 4(a). In order to define the position of valence band maximum (VBM), the energy gap between Fermi level and VBM (ΔEVB) is extracted from the valence-band region. As shown in Fig. 3(b), the ΔEVB values of PVK and PVK:TAPC are 1.05 eV and 1.10 eV, respectively. As a result, via the summation of WF and ΔEVB, the VBM levels of PVK and PVK:TAPC films are calculated to be 5.80 eV and 5.75 eV below the vacuum level, respectively. Fig. 3(d) shows the absorption spectra of PVK and PVK:TAPC, which is converted from Fig. 3(c). The band gaps (Eg) of these two materials could be determined through the absorption onset of the linear region and the Eg values for PVK and PVK:TAPC are found to be 3.64 eV and 3.72 eV, respectively. Therefore, the conduction band minimum (CBM) levels are deduced to be 2.16 eV for PVK and 2.03 eV for PVK:TAPC. It is noted that the HOMO remains nearly unchanged at this blending ratio of PVK to TAPC at 3:1, which slightly influences the hole transport.
To verify the effect of doping TAPC into PVK on the carrier transport, the electron-only device (EOD) (ITO/ZnO/QDs/ZnO/Al) and hole-only device (HOD) (ITO/PEDOT:PSS/HTL/QDs/MoO3/Al) were fabricated. It should be mentioned that the thicknesses of all layers in the above charge-only devices are identical to those used in the working devices. It can be easily found that the current of EOD is much larger than that of HOD with bare PVK as displayed in Fig. 5, because the ZnO NPs are in favor of electron transport due to its similar LUMO level with the CB of QDs (Fig. 1(d)). In contrast, the holes are restricted due to the low hole mobility and shallow HOMO level of PVK, which results in the imbalance of carrier transport. It is anticipated that doping appropriate amount of TAPC into the PVK leads to the high hole mobility. It is clearly reflected in Fig. 5 that the current density of HOD increases with the increased amount of TAPC in PVK and reaches the highest and closest value to the current of EOD when the doping ratio of PVK:TAPC is 3:1. However, when the doping concentration of TAPC increases, the hole transport can be restricted because the film quality will deteriorate as discussed above and the HOMO will decrease due to the comparatively smaller HOMO of TAPC. Thus, it can be speculated that the QLED device with PVK:TAPC (3:1) has the best performance upon the balance of carrier transport attributed to the high hole mobility and appropriate HOMO level of the doped HTL.
Fig. 5 Current–voltage characteristics of the EOD (ITO/ZnO/QD/ZnO/Al) and HODs (ITO/PEDOT:PSS/HTL/QD/MoO3/Al). |
To further verify the effect of doped HTL, QLED devices with different ratios of PVK and TAPC were fabricated. Fig. 6(a) shows higher luminance of QLED with PVK:TAPC (3:1) as doped HTL, indicating the carrier transport is balanced at this condition and it is in favor of the radiative recombination in the EML. At the same time, the HOMO of the doped HTL remains nearly unchanged compared with the bare PVK, which facilitates the hole transport. It is displayed in Fig. 6(a) that both the turn on voltage (3.3 V) of QLED with PVK:TAPC (3:1) as doped HTL and the driving voltage at the highest current efficiency (∼4 V) are lower compared with those (∼6 V and ∼8 V) demonstrated by the other group.35 It is attributed to the carrier balance at this condition due to the enhanced hole transport ability when using the doped HTL, which facilitate the exciton recombination in the EML. In addition, it can be found that the QLEDs with TAPC:PVK = 3:1 show the highest current efficiency and power efficiency of 26.2 cd A−1 and 19.2 lm W−1, i.e. an increase by 55% and 51%, respectively, compared to the device with pristine PVK. It is noted that the efficiencies of the device exceed those of the similar device in the previous work published.25,26 This is because the hole mobility of small molecule used here (TAPC: 1.0 × 10−2 cm2 V−1 s−1) is much higher than that of the small molecule used in other work (TCTA: 2.0 × 10−5 cm2 V−1 s−1). Moreover, the doping ratio of doped HTL has been adjusted carefully to facilitate hole transport and ensure the film quality of the HTL layer, which plays an important role in the film quality of the QDs deposition. All these factors contribute to the performance improvement of QLEDs. In addition, the external quantum efficiency (EQE) of the QLED with PVK:TAPC (3:1) as doped HTL reaches the highest value of 6.2% because of the balanced carrier transport due to the improvement in hole transport ability as displayed in Fig. 6(c). It is worth noting that efficiencies close to the peak value (i.e. EQE ≥90% EQE peak) are maintained in a wide range of brightness of 500–22000 cd m−2. The low efficiency roll-off of this device suggests that our QLEDs are promising for high-power applications. A summary of the QLEDs performance with different HTLs is displayed in Table 2. It is worth noting that when the ratio of PVK and TAPC decreases further, such as 1:1, the performance of the QLED will experience a fast roll-off of efficiency. This is because the film quality will deteriorate when the doping concentration of TAPC is larger due to the relatively low Tg of TAPC as displayed in Fig. 3. Another reason is likely that the HOMO of the doped HTL will become shallower as the doping concentration of TAPC increases excessively, attributing to the small HOMO level of TAPC. Therefore, the performance improvement of the QLED device is attributed to the balance of carrier transport when utilizing the doped HTL, which takes advantage of the superior energy level of PVK and high hole mobility of TAPC. In order to make the conclusion more reliable, a comparison of the average current efficiency of QLEDs with respect to TAPC doping is displayed in Fig. 6(d), considering the device-to-device performance variations. It clearly shows the same variation trend as the single device. In addition, an encouraging high reproducibility of this high performance of our QLEDs was demonstrated by testing 36 devices from 8 batches as shown by the histograms in Fig. 6(e), yielding an average efficiency of 24.1 cd A−1. Electroluminescence (EL) of the device with PVK:TAPC (3:1) as doped HTL at different driving voltage is shown in Fig. 6(f), exhibiting the same EL peak wavelength without peaks from neighbouring organic layers. This demonstrates that the excitons effectively recombine in the QDs layer. The luminescence intensity greatly increases with the increased driving voltage and the device emits the vivid light as shown in the inset of Fig. 6(f). Compared with the PL spectrum, the peak location of the EL spectrum is slightly red-shifted (∼10 nm), which is due to enhanced interdot interactions resulting from the reduced interdot distance in close-packed QDs film, electric-field-induced Stark effect and long-range resonance transfer of electronic excitations from the small to the large dots.36
Device | VT | VD | EQE (%) | CE (cd A−1) | PE (lm W−1) | ||
---|---|---|---|---|---|---|---|
Peak | @1000 cd m−2 | Peak | @1000 cd m−2 | ||||
a VT driving voltage corresponding to 1 cd m−2, VD driving voltage corresponding to 1000 cd m−2. | |||||||
PVK | 3.5 | 4.4 | 4.0 | 16.9 | 16.5 | 12.7 | 11.8 |
PVK:TAPC (5:1) | 3.4 | 4.5 | 4.6 | 19.4 | 17.3 | 13.6 | 13.3 |
PVK:TAPC (4:1) | 3.3 | 4.5 | 5.1 | 21.6 | 18.2 | 13.3 | 12.8 |
PVK:TAPC (3:1) | 3.3 | 4.0 | 6.2 | 26.2 | 24.8 | 19.2 | 19.0 |
PVK:TAPC (2:1) | 3.5 | 4.3 | 3.5 | 14.1 | 13.7 | 12.9 | 10.2 |
PVK:TAPC (1:1) | 3.4 | 4.8 | 2.4 | 10.1 | 8.5 | 7.7 | 5.4 |
In order to further verify the conclusion that device performance improved is attributed to carrier balance, the same method widely used in OLED is adopted to calculate the injection efficiency of hole in our devices. At first, devices with a structure of ITO/PEDOT:PSS/HTL/Au were fabricated to test the hole injection enhancement of the doped HTL device. It is noted that Au was used as cathode here to ensure only the hole transport in these devices. It is found that the device exhibited a great enhancement of current density when the doping ratio of PVK:TAPC is 3:1 as displayed in Fig. 7(a). For instance, the device with the PVK:TAPC (3:1) as doped HTL shows a current density of 10 mA cm−2, larger than that of any other types of devices. The theoretical SCLC displayed in Fig. 7(a) is the calculated current density. Ideally, if an organic material is under condition of ohmic injection contact as well as trap-free, the steady-state current should follow the space-charge-limited current (SCLC) (JSCL):37
(1) |
Fig. 7 (a) J–V characteristics, and (b) hole injection efficiency, ηINJ, of hole-only device as a function of electric field of devices with different HTL. |
The injection efficiency ηINJ can be calculated from the J–V characteristics:40
ηINJ = JINJ/JSCL | (2) |
The hole injection efficiency (ηINJ) curves of different HTL devices is displayed in Fig. 7(b) according to the formula (1) and (2). It can be easily found that the ηINJ increases from 13.2% of the device with PVK as HTL to 40.1%, when adopting the PVK:TAPC (3:1) as doped HTL. Thus, a significant improvement of hole injection efficiency can be obtained using the PVK:TAPC (3:1) as doped HTL, which facilitates the charge balance as well as high performance QLED.
The QLED utilizing the optimized doped HTL exhibits better ambient stability without any encapsulation techniques compared with that with the pristine HTL. For the fair comparison of device lifetime, the constant current of 39 mA cm−2 was applied for the two devices. The device lifetime is estimated by the relation of L0n × T50 = constant (1.5 ≤ n ≤ 2).17 L0 is the initial luminance, 3900 cd m−2 and 4900 cd m−2 for the device with pristine HTL and device with doped HTL and device with doped HTL, respectively. T50 (defined as the time for the luminance reducing to L0/2) is about 9 h and 14 h respectively for the two devices according to Fig. 8. The values of acceleration factor n was assumed as 1.5 according to the literature.17 The device lifetime at initial luminance of 100 cd m−2, calculated by the relation above, is over 2400 and 4000 h for devices with pristine HTL and device with doped HTL, respectively. An enhancement factor of 60% is obtained for the device lifetime when doped HTL is introduced.
This journal is © The Royal Society of Chemistry 2017 |