Ming-Lei Gou*,
Junqing Cai,
Wensheng Song,
Zhen Liu,
Yun-Lai Ren and
Qingshan Niu
School of Chemical Engineering and Pharmaceutics, Henan University of Science and Technology, Luoyang, Henan 471023, PR China. E-mail: mingleigou@haust.edu.cn; Fax: +86 37964231914; Tel: +86 37964231914
First published on 14th September 2017
The performance and coke species of HZSM-5 in the isomerization of styrene oxide to phenylacetaldehyde was investigated under gas phase, free of solvents. The reaction showed higher catalytic stability and phenylacetaldehyde selectivity at around 300 °C, lower feed rate (e.g., WHSV = 1.2–3 h−1) and higher flow rate of carrier gas (e.g., 120 mL min−1). Based on FT-IR spectra, the dimer formed via aldol condensation of phenylacetaldehyde was one of the precursors of coke species. TG results showed that there were two types of coke species. The soft coke, which can be removed via desorption between 200–400 °C, had less influence on the catalytic stability. The hard coke, which had a certain degree of crystallization (i.e., pregraphite-like carbon presenting in XRD patterns) and must be completely removed via burning with oxygen, causes major catalyst deactivation.
(1) |
(2) |
There are two main side reactions in this process: aldol condensation and trimerization of phenylacetaldehyde, as shown in eqn (1) and (2).11 Aldol condensation is not sensitive to the acidity of catalysts and may be a spontaneous process, while trimerization occurs at the external acid sites through an acid-catalyzed process.12 In order to control the side reactions and prevent catalyst deactivation, a large amount of solvents can be used to dilute reactants,7 but the subsequent separation is difficult and the energy consumption extensive. This process can also be operated under gas phase using inert gas (e.g., N2) as carrier gas, which facilitates the transport of reactants and products through the catalyst bed.13 On the premise of styrene oxide conversion, the shorter the contact time is between reactants and catalysts, the lower the probability of side reactions. Particularly, products can be separated in a simple manner without additional purification.
Zeolites are thought to be superior to other catalysts on account of the suppression of side reactions by shape selectivity, particularly the MFI-type zeolites.14 In this study, the catalytic performance of HZSM-5 under different conditions of temperature (200–400 °C), feed rate (weight hourly space velocity, WHSV = 1.2–6.0 h−1) and flow rate of carrier gas (30–120 mL min−1) were firstly examined, then the coke species and deactivation behavior of catalysts under different conditions were analyzed.
Sample | SiO2/Al2O3 (mol mol−1) | BET surface area (m2 g−1) | Pore volume (cm3 g−1) | Pore size Å | Weak acid (mmol g−1) | Strong acid (mmol g−1) | B/L (mol mol−1) | External acid (a.u.) |
---|---|---|---|---|---|---|---|---|
a Reaction conditions: T = 200 °C, P = 1 atm, catalyst loading = 0.5 g, flow rate of N2 = 120 mL min−1, WHSV = 3.0 h−1, 7 h time on stream. | ||||||||
Fresh HZSM-5 | 134.6 | 290.4 | 0.144 | 4.6 | 0.114 | 0.256 | 13.1 | Trace |
Spent HZSM-5a | 135.1 | 15.7 | 0.004 | 1.5 | Trace | 0.120 | 8.9 | Trace |
The powder X-ray diffraction (XRD) patterns were collected on a PANalytical X'Pert Pro diffractometer in the 2θ range of 5–50° with Co Kα radiation source (λ = 0.1789 nm).
The acidic properties of catalysts were measured by temperature-programmed desorption of NH3 (NH3–TPD) and FT-IR spectra of adsorbed pyridine (0.57 nm) and 2,4,6-trimethylpyridine (0.74 nm). NH3–TPD was performed on a conventional apparatus equipped with a thermal conductivity detector. The sample (100 mg, 20–30 mesh) was pretreated at 200 °C in nitrogen and then cooled down to ambient temperature. Sufficient NH3 was supplied into the system, followed by flushing with nitrogen at 150 °C for 1 h. The TPD profile was obtained by heating the sample from 150 to 500 °C at a rate of 15 °C min−1. Simultaneously, the desorbed NH3 was trapped in boric acid and then titrated with a standard H2SO4 solution.15
Brønsted (the band at 1545 cm−1) and Lewis acid sites (the band at 1445 cm−1) on the catalysts were characterized by FT-IR spectra of adsorbed pyridine, and FT-IR spectra with 2,4,6-trimethylpyridine adsorption was used to probe the external acid sites (the band at 1638 cm−1). FT-IR spectra were recorded on a Nicolet 380 spectrometer. The sample was pressed into a self-supporting wafer (diameter: 13 mm, weight: 15 mg) and pretreated at 500 °C for 2 h under vacuum. Probe molecule was adsorbed in situ at ambient temperature and then evacuated at 200 °C for 1 h. Finally, an IR spectrum was recorded, and a difference spectrum was obtained by subtracting the spectrum of the pretreated sample from the spectrum after probe adsorption.
FT-IR spectra of the fresh and spent catalysts were recorded on a Nicolet 380 spectrometer instrument at room temperature. The sample and KBr, with weight ratio of approximately 1:200, were pressed into a tablet and then measured between 400 and 4000 cm−1 with a resolution of 4 cm−1.
The weight loss of the spent catalysts was measured by thermogravimetric analysis (TG-DTA) on a PerkinElmer Pyris 6 thermogravimetric analyzer at a heating rate of 10 °C from room temperature to 800 °C in air or nitrogen flow.
At the end of each experiment, the spent catalyst was unloaded after purging with nitrogen at 200 °C for 2 h to remove any possible residual reactants.
Fig. 1 Influence of temperature on the isomerization of styrene oxide to phenylacetaldehyde. Reaction conditions: P = 1 atm, catalyst loading = 0.5 g, flow rate of N2 = 120 mL min−1, WHSV = 3.0 h−1. |
The main by-products in this reaction were the dimer (2,4-diphenyl-2-butenal) and trimer (2,4,6-tribenzyl-s-trioxane) of phenylacetaldehyde. The dimer was formed via aldol condensation of phenylacetaldehyde (as shown in eqn (1)), while the trimer was formed by trimerization of phenylacetaldehyde through an acid-catalyzed process (as shown in eqn (2)). Some other by-products, such as phenylethanol, phenylethanediol, styrene, and so on, were also detected by GC-MS, with total selectivity values less than 1%.
As shown in Fig. 1, the dimer selectivity remained lower at higher temperatures (such as 350 °C and 400 °C). However, the catalyst lifetime instead decreased as mentioned above. This may be due to the dimer being more readily converted into some high-boiling materials at higher temperature, which deposited on the surface of catalysts, leading to rapid deactivation of catalysts. This can be verified by TG analysis, as discussed in the following section.
For the trimer formation, three adsorbed precursor species should be in adjacent acid sites on the external surface of zeolites. HZSM-5 contained only a trace amount of external acid sites, thus leading to no formation of the trimer at 200–400 °C.
Fig. 2 Influence of feed rate on the isomerization of styrene oxide to phenylacetaldehyde. Reaction conditions: T = 200 °C, P = 1 atm, catalyst loading = 0.5 g, flow rate of N2 = 120 mL min−1. |
The trimerization of phenylacetaldehyde could not happen on HZSM-5 at WHSV = 1.2–6.0 h−1, since the catalyst contained only a trace amount of external acid sites.
Fig. 3 Influence of flow rate of carrier gas on the isomerization of styrene oxide to phenylacetaldehyde. Reaction conditions: T = 200 °C, P = 1 atm, catalyst loading = 0.5 g, WHSV = 3.0 h−1. |
The trimer was not generated on HZSM-5 at the N2 flow rate of 30–120 mL min−1, since it only had trace amount of external acid sites.
The structure of HZSM-5 before and after reaction was examined by XRD, as shown in Fig. 4. The characteristic peaks at 2θ = 9–11° and 26–29° all matched well with typical MFI-type structure (JCPDS-PDF: 00-049-0657). However, a new peak at 2θ = 31.1° (labeled with arrow in Fig. 4) over the spent HZSM-5 was similar to the characteristic peak of graphite at 2θ = 30.7° (JCPDS-PDF: 00-001-0640). This kind of coke can be called pregraphite-like carbon.16 Therefore, the coke species on HZSM-5 from the isomerization of styrene oxide to phenylacetaldehyde has a certain degree of crystallization.
Fig. 4 XRD patterns of the fresh and spent HZSM-5. Reaction conditions: T = 200 °C, P = 1 atm, catalyst loading = 0.5 g, flow rate of N2 = 120 mL min−1, WHSV = 3.0 h−1, 7 h time on stream. |
To obtain information on the nature of the coke species, FT-IR spectra of the fresh and spent HZSM-5 were investigated. There were two important regions against the characteristic bands of coke: (i) 2800–3100 cm−1 (as shown in Fig. 5(A)), and (ii) 1300–1700 cm−1 (as shown in Fig. 5(B)). In the range of 2800–3100 cm−1, the bands at 2870 cm−1 and 2925 cm−1 were assigned to the symmetric vibrations of –CH2 or –CH3 and the asymmetric vibration of –CH2.17 Taking into account the absence of the band at 2955 cm−1 (the asymmetric vibration of CH3), the band at 2870 cm−1 can be identified as the symmetric vibrations of –CH2. The bands beyond 3000 cm−1 usually belong to C–H stretching vibrations in unsaturated hydrocarbons. For instance, the bands at 3029 cm−1 and 3063 cm−1 were associated with the single-ring or alkyl aromatics,18 and the band at 3086 cm−1 was attributed to olefinic –CH groups.19 It is known that among the main products of this process, only the dimer (2,4-diphenyl-2-butenal) contained olefinic –CH groups. Thus, the aldol condensation of phenylacetaldehyde is one of the factors leading to coke formation in the isomerization of styrene oxide.
In the range of 1300–1700 cm−1, the distinct bands at 1453 cm−1 and 1495 cm−1 are due to benzene skeleton vibration,20 and the bands at 1506 cm−1 and 1540 cm−1 can be assigned to ring stretching and CC stretching vibrations in alkyl or poly aromatics.21,22 It can be deduced that the aromatic-type of carbonaceous compounds were formed on the surface of zeolites. There were also three small bands at 1472 cm−1, 1521 cm−1 and 1559 cm−1, which were assigned to deformation vibrations of –CH or –CH2 groups and CC stretching vibrations of alkenes,23,24 thus again confirming that the dimer formed via aldol condensation of phenylacetaldehyde was one of the precursors for coke formation. However, the absence of the characteristic band of carbonyl group at around 1750 cm−1 implied that the dimer would then convert to polyaromatics and even the pregraphite-like carbon on the surface of HZSM-5.
Weight loss of the spent catalysts at different reaction conditions was measured by TG, as listed in Table 2. The weight loss can be divided into three stages: stage I (<200 °C) was ascribed to the volatilization of adsorbed water and some volatile species, and stage II (200–400 °C) and stage III (400–700 °C) were ascribed to the desorption or combustion of coke species. The weight loss in stage II (so-called soft coke) varied slightly with different reaction conditions and was between 4.3–5.8%, while the weight loss in stage III (so-called hard coke) presented an obvious change as the temperature, feed rate and flow rate of N2 changed. From the above results, temperature, feed rate and flow rate of N2 all had obvious impacts on the catalytic stability and product distribution. Therefore, it is assumed that the soft coke has less influence on the catalytic stability, while the hard coke, which is the more polymerized coke species, would cause major catalyst deactivation.
Spent catalyst | Coke (wt%) | ||
---|---|---|---|
Soft coke (200–400 °C) | Hard coke (400–700 °C) | Total | |
a HZSM-5-T-200/250/300/350/400-7h means the reaction is carried out at 200, 250, 300, 350 or 400 °C with 7 h time on stream; other conditions are: P = 1 atm, catalyst loading = 0.5 g, flow rate of N2 = 120 mL min−1, WHSV = 3.0 h−1.b HZSM-5-W-1.2/6.0-7h means the reaction is carried out at WHSV = 1.2, 6.0 h−1 with 7 h time on stream; other conditions are: T = 200 °C, P = 1 atm, catalyst loading = 0.5 g, flow rate of N2 = 120 mL min−1.c HZSM-5-F-30/60-6h means the reaction is carried out at flow rate of N2 = 30, 60 mL min−1 with 7 h time on stream; other conditions are: T = 200 °C, P = 1 atm, catalyst loading = 0.5 g, WHSV = 3.0 h−1.d HZSM-5-T-200-7h-nitrogen means the TG analysis is operated in nitrogen atmosphere, reaction conditions are: T = 200 °C, P = 1 atm, catalyst loading = 0.5 g, flow rate of N2 = 120 mL min−1, WHSV = 3.0 h−1, 7 h time on stream. | |||
HZSM-5-T-200-7ha | 5.6% | 5.9% | 11.5% |
HZSM-5-T-250-7h | 5.1% | 4.1% | 9.2% |
HZSM-5-T-300-7h | 4.8% | 3.6% | 8.4% |
HZSM-5-T-350-7h | 4.9% | 4.5% | 9.4% |
HZSM-5-T-400-7h | 5.0% | 4.9% | 9.9% |
HZSM-5-W-1.2-7hb | 4.3% | 3.7% | 8.0% |
HZSM-5-W-6.0-7h | 5.8% | 7.8% | 13.6% |
HZSM-5-F-30-7hc | 5.7% | 6.6% | 12.3% |
HZSM-5-F-60-7h | 5.7% | 6.3% | 12.0% |
HZSM-5-T-200-7h-nitrogend | 5.8% | 2.7% | 8.5% |
As shown in Table 2, the amount of hard coke first decreased and then increased as the temperature increased from 200 °C to 400 °C, which was converse to the change in catalyst lifetime as shown in Fig. 1. Based on the FT-IR analysis, the dimer was one of the precursors for coke formation. The dimer selectivity remained lower at higher temperature (i.e., 350 °C and 400 °C); simultaneously, the amount of hard coke increased, and the catalyst lifetime decreased. So it can be verified from the above that the dimer more readily converts to some high-boiling materials at higher temperature, which deposit on the surface of the catalyst, resulting in a larger amount of hard coke and rapid deactivation of catalysts.
From Fig. 2 and 3, the dimer selectivity values increased and the catalyst lifetime decreased at higher feed rate (e.g., WHSV = 6.0 h−1) and lower N2 flow rate (e.g., 30 mL min−1). Based on the TG analysis in Table 2, the amount of hard coke increased as feed rate increased and N2 flow rate decreased. Therefore, it can be confirmed that the probability of side reactions (i.e., the aldol condensation) increases with longer contact time at higher feed rate and lower N2 flow rate, which accelerates the coke formation and deactivation of catalysts.
It is well known that most of the acid sites on HZSM-5 exist inside the micropores; thus, the catalytic stability is mainly determined by the reactions occurring at the internal acid sites. From FT-IR spectra and TG analysis, the dimer formed via aldol condensation of phenylacetaldehyde is one of the precursors of coke species. The dimer can then convert to some high-boiling materials (so-called hard coke), which would cause major catalyst deactivation, while the trimer is not responsible for the deactivation of HZSM-5.
As shown in Table 2, weight loss differences of the spent HZSM-5 in air and nitrogen atmosphere were also observed. The weight loss at stage II was similar whether in air (5.6%) or nitrogen (5.8%), showing that this soft coke can be completely removed via desorption from the catalysts between 200–400 °C. However, the weight loss at stage III in nitrogen atmosphere (2.7%) was lower than that in air (5.9%), indicating that this hard coke must be completely removed with oxygen. The weight loss above 700 °C in nitrogen was approximately 1.6%, which was due to part of the hard coke slowly decomposing to some volatile species. On the basis of XRD, the coke formation on HZSM-5 has a certain degree of crystallization, i.e., pregraphite-like carbon, which also has to be removed via burning with oxygen. By comparing the weight loss in air or nitrogen atmosphere, approximately 1.6% of the pregraphite-like carbon was formed on HZSM-5 in the isomerization of styrene oxide to phenylacetaldehyde at 200 °C, WHSV = 3.0 h−1 and N2 flow rate = 120 mL min−1.
This journal is © The Royal Society of Chemistry 2017 |