Jonna Hynynen,
David Kiefer and
Christian Müller*
Department of Chemistry and Chemical Engineering, Chalmers University of Technology, 41296 Göteborg, Sweden. E-mail: christian.muller@chalmers.se
First published on 4th January 2018
Doping of the conjugated polymer poly(3-hexylthiophene) (P3HT) with the p-dopant 2,3,5,6-tetrafluoro-7,7,8,8-tetracyanoquinodimethane (F4TCNQ) is a widely used model system for organic thermoelectrics. We here study how the crystalline order influences the Seebeck coefficient of P3HT films doped with F4TCNQ from the vapour phase, which leads to a similar number of F4TCNQ anions and hence (bound + mobile) charge carriers of about 2 × 10−4 mol cm−3. We find that the Seebeck coefficient first slightly increases with the degree of order, but then again decreases for the most crystalline P3HT films. We assign this behaviour to the introduction of new states in the bandgap due to planarisation of polymer chains, and an increase in the number of mobile charge carriers, respectively. Overall, the Seebeck coefficient varies between about 40 to 60 μV K−1. In contrast, the electrical conductivity steadily increases with the degree of order, reaching a value of more than 10 S cm−1, which we explain with the pronounced influence of the semi-crystalline nanostructure on the charge-carrier mobility. Overall, the thermoelectric power factor of F4TCNQ vapour-doped P3HT increases by one order of magnitude, and adopts a value of about 3 μW m−1 K−2 in the case of the highest degree of crystalline order.
(1) |
(2) |
Conjugated polymers are of particular interest because a wide range of rheological and mechanical properties can be selected through careful choice of the molecular weight. Further, many conjugated polymers now offer a high charge-carrier mobility μ, which is needed to reach a high electrical conductivity according to:
σ = nqμ | (3) |
Fig. 1 Schematic of home-built vapour doping chamber with the dimensions 20 × 15 × 10 mm; chemical structure of P3HT and F4TCNQ; schematic reproduced with permission from ref. 18; copyright the American Chemical Society 2017. |
The dopant can be introduced by two means, either through co-processing together with the polymer from the same solution,6,7,11–13 which leads to aggregation that disrupts the solid-state order of P3HT,14 or through sequential doping.14–17 Sequential doping can be carried out by either depositing the dopant onto the polymer from the vapour phase (‘vapour doping’),15,18 or by bringing the polymer in contact with an orthogonal solvent that dissolves the dopant.14,16,17 Sequential doping is of interest since it allows to circumvent the aggregation of P3HT that occurs during co-processing. Instead, the nanostructure of the polymer can develop under controlled conditions. Subsequently, P3HT can be doped in a precise manner, which allows to study the interplay of charge-carrier density, nanostructure and electrical properties.17–19 Moreover, sequential doping can lead to a significantly higher electrical conductivity above 10 S cm−1.17,18
Recently, we as well as others have studied the influence of the crystallinity on the electrical conductivity of sequentially doped P3HT.18–20 By tuning the regioregularity and processing solvent the nanostructure of P3HT could be altered leading to a much higher electrical conductivity. For example, by changing the polymer processing solvent we were able to increase the electrical conductivity from 0.01 to 13 S cm−1, which we attributed to the higher charge-carrier mobility that resulted from a higher degree of polymer crystallinity.18 Similar findings were made by Scholes et al.19 and Chew et al.20 who concluded that the ordered regions of P3HT give rise to a higher charge-carrier mobility and therefore lead to an increase in the electrical conductivity. Here, we explore how the crystallinity influences the power factor of P3HT vapour-doped with F4TCNQ. We find that an increase in the crystalline order enhances the power factor by one order of magnitude from 0.2 to 2.7 μW m−1 K−2.
To compare the degree of solid-state order of neat P3HT films, we recorded UV-vis absorbance spectra. We fitted the spectra according to the model developed by Spano et al., assuming a Huang–Rhys factor of 1:21–23
(4) |
Fig. 2 Representative UV-vis absorption spectra of neat P3HT films spincoated from various solvents at 60 °C (purple symbols), and films vapour doped for 3 min (green symbols); spectra of neat P3HT are fitted according to ref. 21–23; spectra of doped P3HT are fitted according to ref. 11 and 24, and are composed of (1) two Gaussians representing the contribution from polaron absorption centered at 1.33 eV and 1.67 eV, respectively (green), (2) P3HT aggregate absorption modelled according to ref. 21–23 (not shown), and (3) measured absorption spectrum of the F4TCNQ anion (orange) ref. 24. |
We then doped the neat P3HT films by exposing them to vapour of F4TCNQ at ambient conditions as previously described (for vapour doping setup see Fig. 1).18 The degree of doping correlates with the period of time that the samples are exposed to F4TCNQ vapour. For the vapour-doped samples, we find that the conductivity sharply increases during the first two minutes of doping but then levels off for longer doping times (Table 1). We therefore selected a doping time of 3 min to compare samples spincoated from different solvents. For the least ordered samples spincoated from chloroform we find an electrical conductivity of only 0.7 S cm−1, whereas more highly ordered p-xylene films yielded a value of 12.7 S cm−1 after 3 min of doping. We have demonstrated previously that the electrical conductivity increases with the degree of crystalline order of P3HT, as evidenced by the inverse correlation of σ and W (Fig. 3).18
Solvent | tvapour (min) | σ (S cm−1) | α (μV K−1) |
---|---|---|---|
Chlorobenzene/o-dichlorobenzene | 0.5–2 | 0.6 ± 1.3 | 62 ± 17 |
2.5–5 | 5.5 ± 2.0 | 54 ± 4 | |
10 | 2.9 ± 2.3 | 57 ± 4 | |
p-Xylene | 0.5–2 | 5.0 ± 5.4 | 54 ± 11 |
2.5–5 | 12.7 ± 2.8 | 43 ± 3 | |
10 | 14.5 ± 0.5 | 48 ± 2 |
Fig. 3 (a) Electrical conductivity σ as a function of free exciton bandwidth W, calculated by fitting UV-vis spectra according to ref. 21–23: (b) charge-carrier mobility μ as a function of free exciton bandwidth W. |
We explain the correlation between conductivity and crystallinity with the well-established impact of the former on the charge-carrier mobility. We can use eqn (3) to estimate the mobility if we can determine the number of charge carriers. Since doping of P3HT with F4TCNQ occurs through integer charge transfer, we assume that each F4TCNQ anion corresponds to one charge on the polymer. We here do not distinguish between bound and free charge carriers and instead consider the average mobility. Therefore, we equate the F4TCNQ anion concentration with the number of charge carriers. We estimate the anion concentration by fitting UV-vis spectra of doped films according to a procedure first proposed by Wang et al.24 For all six processing solvents we extract a similar value of about 2 × 10−4 mol cm−3, which corresponds to 0.03 anions per P3HT repeat unit (or 4.7 wt% anions assuming a density of 1 g cm−3). Based on this value we find that for the here studied samples the mobility increases from 0.05 to 0.5 cm2 V−1 s−1 (Fig. 3). Pingel et al. have shown for F4TCNQ-doped P3HT that only a fraction of anions gives rise to free charge carriers,25 which implies that our mobility estimate represents a lower bound.
The Seebeck coefficient, instead, shows a markedly different, non-monotonic behaviour. For the most disordered samples, spincoated from chloroform, we measure a low Seebeck coefficient of 51 μV K−1 (Table 2). For more ordered samples we find a slightly higher value of 60 μV K−1, whereas the most ordered samples, spincoated from p-xylene, display the lowest Seebeck coefficient of 43 μV K−1. In case of poly(3,4-ethylenedioxythiophene):tosylate (PEDOT:Tos) with a constant dopant concentration the Seebeck coefficient has been shown to slightly increase with the degree of crystalline order.26 Fabiano et al. argue that the slight increase in Seebeck coefficient from 32 to 44 μV K−1 arises because of a steeper density of states at the Fermi level, caused by the presence of states in the bandgap as a result of delocalisation in ordered domains. Since the charge-carrier mobility likewise improves through the presence of ordered domains, a correlation between the Seebeck coefficient and mobility is observed for PEDOT:Tos. We argue that a similar behaviour results in the slight increase in Seebeck coefficient that we observe for more disordered samples, e.g. when changing the spincoating solvent from chloroform to chlorobenzene (Table 2).
Solvent | W (meV) | Aggregates (%) | σ (S cm−1) | α (μV K−1) | F4TCNQ anion conc. (10−4 mol cm−3) |
---|---|---|---|---|---|
Chloroform | 155 | 33 | 0.7 ± 0.4 | 51 ± 2 | 2.3 ± 0.3 |
Chlorobenzene | 110 | 38 | 2.0 ± 0.7 | 63 ± 1 | 2.9 ± 0.6 |
Toluene | 58 | 42 | 5.3 ± 2.1 | 55 ± 4 | 2.1 ± 0.4 |
Chlorobenzene/o-dichlorobenzene | 64 | 42 | 6.1 ± 0.8 | 59 ± 3 | 1.9 ± 0.4 |
1,2,4-Trichlorobenzene | 54 | 43 | 5.6 ± 0.6 | 56 ± 2 | 1.7 ± 0.3 |
p-Xylene | 30 | 46 | 12.7 ± 2.8 | 46 ± 2 | 3.0 ± 0.6 |
The slight decrease in Seebeck coefficient that we observe for more ordered samples may arise because of an increase in the number of mobile charge carriers. The Seebeck coefficient predominately probes mobile charge carriers and therefore a change in their concentration will influence the measured thermovoltage. We note that the concentration of F4TCNQ anions does not change with the degree of order. Therefore, we deem it likely that the same number of charges are generated per volume of amorphous and crystalline phase. However, the mobility of charges may depend on the local order in the vicinity where a particular charge is generated. Gao et al. have argued that both regiorandom and regioregular P3HT can interact with F4TCNQ when dissolved in a common solvent.27 However, only in case of regioregular P3HT free charges are generated because the polymer is readily able to adopt a planar conformation, which facilitates delocalisation of hole charges. In our samples, both disordered, amorphous and ordered, crystalline domains are present. Doping of P3HT in crystalline domains readily leads to a free charge because the polymer is already planarised. Instead, doping of P3HT in amorphous domains requires that the polymer chain adopts a more planar conformation upon doping. Consistent with this picture, Chew et al. have recently proposed that for sequentially doped P3HT the film connectivity is improved because doping leads to more extended P3HT crystallites.20 We argue that molecular motion in amorphous domains is more restricted than in a dilute polymer solution, discussed in the work by Gao et al.,27 and therefore doping cannot readily induce the same degree of order that is already present in crystalline domains. The presence of structural defects implies that at least some charges are bound. Hence, we anticipate that the amount of mobile charges increases with the initial crystallinity of P3HT, leading to a reduction of the Seebeck coefficient, which may explain the slightly lower value that we measured for the most ordered samples spincoated from p-xylene.
Finally, we compare our results with other reports for a number of different polythiophenes, including P3HT, the copolymer poly(bithiophene-alt-thienothiophene) (PBTTT) and the oligo ethylene glycol bearing derivative p(g42T-T) (Fig. 4).6,11,17,28–37 The variation in Seebeck coefficient with electrical conductivity follows the empirical trend described by eqn (2) (Fig. 4, top). Data points that lie to the left of this empirical line are thought to be mobility limited: a given degree of doping results in a certain Seebeck coefficient, but many charges cannot traverse the material sufficiently quickly because their motion is impeded by structural defects. One illustrative example are ternary blends of P3HT:F4TCNQ with poly(ethylene oxide) (PEO). We have found that in case of a sufficiently high concentration of P3HT:F4TCNQ the Seebeck coefficient and electrical conductivity follow the empirical trend of eqn (2).11 In contrast, in case of more dilute blends the connectivity between P3HT:F4TCNQ domains is poor, leading to a lower mobility and hence electrical conductivity (cf. red filled circles in Fig. 4). We note that the conductivity that we have measured for samples spincoated from chloroform diverges from the empirical trend of eqn (2). We assign this behaviour to the low charge-carrier mobility that we deduce for these samples, caused by poor connectivity of crystalline domains.
Fig. 4 Seebeck coefficient α (top) and power factor α2σ (bottom) as a function of electrical conductivity σ measured in this study (red stars), and extracted from literature: P3HT doped with F4TCNQ (filled red squares),6,17,28 NOPF6 (red crosses),29 FTS or TFSI (open red triangles),6,30–32 or FeCl3 (open red diamonds);33 P3HT:PEO doped with F4TCNQ (filled red circles);11 P3HT:P3HTT doped with F4TCNQ (open red circles);34 PBTTT doped with F4TCNQ (filled blue squares),6,35 FTS or TFSI (open blue triangles),6,30,36 or F2TCNQ (open blue squares);35 and p(g42T-T) doped with F4TCNQ or DDQ (open crossed circles);37 the dashed lines are drawn according to eqn (2) [FTS = (tridecafluoro-1,1,2,2-tetrahydrooctyl)trichlorosilane; TFSI = Fe(III)triflate; P3HTT = poly(3-hexylthiothiophene); PBTTT = poly(2,5-bis(3-tetradecylthiophen-2-yl)thieno[3,2-b]thiophene); F2TCNQ = 2,5-difluoro-7,7,8,8-tetracyanoquinodimethane; DDQ = 2,3-dichloro-5,6-dicyano-p-benzoquinone]. |
The opposite case are samples that are mobility enhanced, where charges are able to traverse the material more quickly than predicted by the empirical trend of eqn (2), leading to a higher conductivity for a given Seebeck coefficient. An example is the recent work by Brinkmann et al., who studied sequentially-doped P3HT films that had been uniaxially aligned through rubbing.17 Upon F4TCNQ doping a concomitant increase in electrical conductivity and Seebeck coefficient was observed, with maximum values of σ = 22 S cm−1 for α = 60 μV K−1, which we rationalise with improved connectivity along the direction of orientation.
Fig. 5 (a) Power factor α2σ as a function of free exciton bandwidth W calculated by fitting UV-vis spectra according to ref. 21–23, and (b) power factor α2σ as a function of average charge-carrier mobility μ. |
This journal is © The Royal Society of Chemistry 2018 |